Welding rod for repair welding of high manganese steel frog

By adding specific alloy elements and welding process optimization to the welding rod for welding replenishment of high manganese steel, the problems of low tensile strength and elongation after break are solved, and the high hardness and resistance of high manganese steel are achieved The cracking performance meets the high strength and plastic toughness requirements for the repair of the tramp during service.

CN118926768AActive Publication Date: 2024-11-12TIANJIN YONGCHANG WELDING WIRES +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411329637.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

The tensile strength and elongation after breaking of the existing fork welding replenishment electrodes are low, which cannot meet the needs of repairing defects such as wear, cracks, block drops, collapses and other defects during service of high-manganese steel forks.

Method used

High manganese steel fork welding and repair welding rods are used. The welding rods include welding cores and powders coated on the surface of the welding core. The welding cores and powders are composed of specific mass percentages, and elements such as C, Mn, Cr, Mo, Si are added to the alloy. The interaction of elements, adjust the appropriate content to obtain excellent comprehensive mechanical properties, no preheating during welding, arc welding, current and welding speed are controlled within a specific range.

Benefits of technology

The high hardness of the welding rod, tensile strength ≥750MPa, elongation after break ≥40%, and impact work at room temperature ≥70J, meeting the high strength and plastic toughness requirements of the junction, and improving the low-temperature deformation stability and resistance of the weld structure Corrosion capability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a welding rod for repair welding of a high-manganese steel frog. The welding rod comprises a core wire and powder wrapping the surface layer of the core wire. Wherein the powder comprises the following components in percentage by mass: 30-40% of marble, 4-8% of fluorite, 2-5% of silica powder, 25-45% of manganese metal, 3-8% of rutile, 0.5-1% of sodium carbonate, 5-10% of chromium powder, 2-5% of molybdenum powder, 3-6% of nickel powder, 1-3% of graphite and 1-3% of roasted mica; the core wire comprises, by mass, less than or equal to 0.10% of C, 0.40-0.65% of Mn, less than or equal to 0.030% of Si, less than or equal to 0.030% of S, less than or equal to 0.030% of P, less than or equal to 0.20% of Cr, less than or equal to 0.30% of Ni and less than or equal The excellent comprehensive mechanical property is obtained by adjusting the proper content of different alloy elements, and it is guaranteed that the room-temperature structure of deposited metal of the welding rod is austenite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding materials, and in particular relates to a welding rod for repairing high manganese steel frog welding. Background Art

[0002] With the rapid development of my country's railways, the speed of railway operation is constantly increasing, the operation density is also increasing, and the requirements for the quality of rail products are getting higher and higher. As an important structural part of the rail, the quality of the frog is also an important factor affecting the development of railways. Therefore, there are also higher quality requirements for the frog.

[0003] Railway frogs are mostly made of high manganese steel. However, during the service life of railway high manganese steel frogs, defects such as surface wear, cracks, block drop, collapse, and crushing are prone to occur, and the frogs need to be repaired by welding. Therefore, it is necessary to put forward quality requirements for welding materials, that is, in addition to having a certain wear resistance and crack resistance, they should also have high strength and plastic toughness. In the prior art, the tensile strength and elongation of the frog welding rods are relatively low. Summary of the invention

[0004] In view of this, the present invention aims to overcome the defects in the prior art and provides a high manganese steel frog welding repair electrode and a welding method.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] In a first aspect, the present invention provides a high manganese steel frog welding repair electrode, the electrode of the present invention comprises a welding core and a powder coated on the surface of the welding core;

[0007] The powder is composed of the following by mass percentage: 30-40% marble, 4-8% fluorite, 2-5% silicon powder, 25-45% metallic manganese, 3-8% rutile, 0.5-1% soda ash, 5-10% chromium powder, 2-5% molybdenum powder, 3-6% nickel powder, 1-3% graphite and 1-3% roasted mica.

[0008] The welding core has the following compositions by mass percentage: C≤0.10%, Mn 0.40-0.65%, Si≤0.030%, S≤0.030%, P≤0.030%, Cr≤0.20%, Ni≤0.30%, Cu≤0.20%, and the balance is Fe.

[0009] The deposited metal of the high manganese steel frog welding rod comprises the following components in weight percentage: C 0.15-0.35%, Mn 12.0-18.0%, Cr 3.0-5.0%, Ni 2.0-5.0%, Mo 1.0-2.0%, Si≤0.30%, S≤0.020%, P≤0.030%, and the balance is Fe and unavoidable impurities.

[0010] Among them, the C element is a strong austenitizing element: C atoms exist in the form of interstitial atoms in austenite, and are a stable austenite element. They play a significant role in solid solution strengthening, enhancing the strength of the austenite matrix, improving the low-temperature deformation stability of the weld structure, and improving the strength of the weld metal. If the C content is low, the weld hardness will not meet the use requirements, and when the C content is too high, it is easy to cause the weld to become brittle and crack.

[0011] Mn is an austenitizing element that can form an infinite substitution solid solution in austenite and has a solid solution strengthening effect. Mn, supplemented with other alloying elements such as C and Ni, can keep austenite stable at room temperature. Too much Mn will reduce the tensile strength and yield strength, while too low Mn will not ensure the retention of the full austenite structure at room temperature, so it is necessary to control the appropriate content of Mn.

[0012] The addition of Cr will distort the austenite lattice, produce a solid solution strengthening effect, and facilitate the precipitation of carbides in the austenite matrix, producing second phase strengthening. In addition, the addition of Cr can improve the corrosion resistance of high manganese steel.

[0013] Mo is an austenitizing element, which helps to improve the growth tendency of dendrites and significantly improve the morphology, quantity and distribution of carbides, making it easier to obtain a deeper hardening depth.

[0014] The Si element acts as a deoxidizer in high manganese steel, playing a role in solid solution strengthening and improving yield strength. However, too high Si content can easily cause high manganese steel to form coarse grains, which has an adverse effect on mechanical properties.

[0015] Preferably, the deposited metal has a tensile strength of ≥750 MPa, an elongation after fracture of ≥40%, an impact energy at room temperature of ≥70 J, and a Brinell hardness of ≥200 HBW.

[0016] In the second aspect, the present invention also provides a welding method using the above-mentioned high manganese steel frog welding rod for welding, comprising the following steps: 1) no preheating before welding, the interpass temperature is 90-100°C; 2) using electrode arc welding, the welding current is 120A-160A, and the welding speed is 2.5-5.5mm / s.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] (1) The deposited metal of the high manganese steel frog welding rod of the present invention has reduced C content and Mn content, and simultaneously adds elements such as Cr, Mo, and Ni. Since the influence of alloying elements on the mechanical properties of materials has a significant interaction, the present invention obtains excellent comprehensive mechanical properties by adjusting the appropriate content of different alloying elements, and ensures that the room temperature microstructure of the deposited metal of the welding rod is austenite.

[0019] (2) The alloy elements in the deposited metal of the high manganese steel frog welding rod of the present invention interact with each other and have a common influence on each other, thereby ensuring high hardness while also having excellent comprehensive mechanical properties, with a tensile strength of ≥750MPa, an elongation after fracture of ≥40%, an impact energy at room temperature of ≥70J, and a Brinell hardness of ≥200HBW. DETAILED DESCRIPTION

[0020] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0021] The present invention is described in detail below in conjunction with embodiments.

[0022] Example 1

[0023] A welding rod for repairing high manganese steel frog welding, comprising a welding core and powder coated on the surface of the welding core;

[0024] The powder is composed of the following by mass percentage: marble 35%, fluorite 6.5%, silica powder 2%, metallic manganese 32%, rutile 5%, soda ash 0.8%, chromium powder 8%, molybdenum powder 3%, nickel powder 4.5%, graphite 1.2%, and roasted mica 2%;

[0025] The welding core has the following compositions by mass percentage: C 0.075%, Mn 0.48%, Si 0.025%, S 0.005%, P 0.012%, Cr 0.035%, Ni 0.023%, Cu 0.018%, and the balance is Fe.

[0026] Welding method: welding current 150A, interpass temperature 90-100℃, welding speed 2.8mm / s.

[0027] The deposited metal of the welding rod has the following composition by mass percentage: C 0.17%, Mn 13.21%, Cr 4.82%, Ni 4.43%, Mo 1.73%, Si 0.12%, S 0.005%, P 0.015%, and the rest is Fe and unavoidable impurities.

[0028] Mechanical properties of deposited metal: tensile strength 795MPa, elongation after fracture 40%, room temperature impact energy 82J, hardness 216HBW.

[0029] Example 2

[0030] A welding rod for repairing high manganese steel frog welding, comprising a welding core and powder coated on the surface of the welding core;

[0031] The composition of the powder is as follows by mass percentage: 30% marble, 5% fluorite, 2% silica powder, 43% metallic manganese, 3% rutile, 1% soda ash, 6.5% chromium powder, 2% molybdenum powder, 3% nickel powder, 3% graphite, and 1.5% roasted mica;

[0032] The welding core has the following compositions by mass percentage: C 0.075%, Mn 0.48%, Si 0.025%, S 0.005%, P 0.012%, Cr 0.035%, Ni 0.023%, Cu 0.018%, and the balance is Fe.

[0033] Welding method: welding current 140A, interpass temperature 90-100℃, welding speed 3.8mm / s.

[0034] The composition of the electrode deposited metal, by mass percentage, is as follows: C 0.32%, Mn 17.26%, Cr 3.75%, Ni2.78%, Mo 1.23%, Si 0.12%, S 0.005%, P 0.014%, and the rest is Fe and unavoidable impurities.

[0035] Mechanical properties of deposited metal: tensile strength 819MPa, elongation after fracture 43.5%, impact energy at room temperature 90J, hardness 224HBW.

[0036] Example 3

[0037] A welding rod for repairing high manganese steel frog welding, comprising a welding core and powder coated on the surface of the welding core;

[0038] The composition of the powder by mass percentage is as follows: marble 32%, fluorite 4%, silica powder 2%, metallic manganese 38%, rutile 6%, soda ash 0.5%, chromium powder 7%, molybdenum powder 2.5%, nickel powder 3.5%, graphite 2.5%, roasted mica 2%;

[0039] The welding core has the following compositions by mass percentage: C 0.075%, Mn 0.48%, Si 0.025%, S 0.005%, P 0.012%, Cr 0.035%, Ni 0.023%, Cu 0.018%, and the balance is Fe.

[0040] Welding method: welding current 160A, interpass temperature 90-100℃, welding speed 3.8mm / s.

[0041] The deposited metal of the welding rod has the following composition by mass percentage: C 0.24%, Mn 15.93%, Cr 4.18%, Ni 3.11%, Mo 1.47%, Si 0.14%, S 0.004%, P 0.015%, and the rest is Fe and unavoidable impurities.

[0042] Mechanical properties of deposited metal: tensile strength 806MPa, elongation after fracture 42%, room temperature impact energy 85J, hardness 229HBW.

[0043] Comparative Example 1

[0044] A welding rod for repairing high manganese steel frog welding, comprising a welding core and powder coated on the surface of the welding core;

[0045] The composition of the powder by mass percentage is as follows: marble 28%, fluorite 3%, silica powder 3%, metallic manganese 36%, rutile 2%, soda ash 1%, chromium powder 12%, molybdenum powder 5.5%, nickel powder 3.8%, graphite 4.5%, and roasted mica 1.2%;

[0046] The welding core has the following compositions by mass percentage: C 0.075%, Mn 0.48%, Si 0.025%, S 0.005%, P 0.012%, Cr 0.035%, Ni 0.023%, Cu 0.018%, and the balance is Fe.

[0047] Welding method: welding current 160A, interpass temperature 90-100℃, welding speed 3.0mm / s.

[0048] The deposited metal of the electrode has the following composition by mass percentage: C 0.48%, Mn 15.42%, Cr 5.71%, Ni 3.29%, Mo 2.78%, Si 0.24%, S 0.005%, P 0.017%, and the rest is Fe and unavoidable impurities.

[0049] Mechanical properties of deposited metal: tensile strength 837MPa, elongation after fracture 30%, impact energy at room temperature 60J, hardness 175HBW.

[0050] Comparative Example 2

[0051] A welding rod for repairing high manganese steel frog welding, comprising a welding core and powder coated on the surface of the welding core;

[0052] The composition of the powder by mass percentage is as follows: 25% marble, 5% fluorite, 2% silica powder, 55% metallic manganese, 3% rutile, 1% soda ash, 3% chromium powder, 1.5% molybdenum powder, 1.5% nickel powder, and 3% roasted mica;

[0053] The welding core has the following compositions by mass percentage: C 0.075%, Mn 0.48%, Si 0.025%, S 0.005%, P 0.012%, Cr 0.035%, Ni 0.023%, Cu 0.018%, and the balance is Fe.

[0054] Welding method: welding current 160A, interpass temperature 90-100℃, welding speed 3.0mm / s.

[0055] The composition of the electrode deposited metal, by mass percentage, is as follows: C 0.066%, Mn 22.26%, Cr 1.30%, Ni 1.3%, Mo 0.75%, Si 0.32%, S 0.004%, P 0.015%, and the rest is Fe and unavoidable impurities.

[0056] Mechanical properties of deposited metal: tensile strength 694MPa, elongation after fracture 20%, room temperature impact energy 77J, hardness 168HBW.

[0057] The mechanical properties of Examples 1-3 and Comparative Examples 1-2 are compared in Table 1:

[0058] Table 1 Mechanical properties

[0059] project Tensile strength MPa Elongation after break % Impact energy J Hardness HBW Example 1 795 40 82 216 Example 2 819 43.5 90 224 Example 3 806 42 85 229 Comparative Example 1 837 30 60 255 Comparative Example 2 694 20 77 168

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high manganese steel frog welding repair electrode, characterized in that: It includes a welding core and powder coated on the surface of the welding core; The powder is composed of the following by mass percentage: 30-40% marble, 4-8% fluorite, 2-5% silica powder, 25-45% manganese metal, 3-8% rutile, 0.5-1% soda ash, 5-10% chromium powder, 2-5% molybdenum powder, 3-6% nickel powder, 1-3% graphite, and 1-3% roasted mica; The welding core has the following compositions by mass percentage: C≤0.10%, Mn 0.40-0.65%, Si≤0.030%, S≤0.030%, P≤0.030%, Cr≤0.20%, Ni≤0.30%, Cu≤0.20%, and the balance is Fe.

2. The high manganese steel frog welding repair electrode according to claim 1, characterized in that: The deposited metal of the high manganese steel frog welding rod comprises the following components in weight percentage: C 0.15-0.35%, Mn 12.0-18.0%, Cr 3.0-5.0%, Ni 2.0-5.0%, Mo1.0-2.0%, Si≤0.30%, S≤0.020%, P≤0.030%, and the balance is Fe and unavoidable impurities.

3. The high manganese steel frog welding repair electrode according to claim 1, characterized in that: The deposited metal has a tensile strength of ≥750MPa, an elongation after fracture of ≥40%, an impact energy at room temperature of ≥70J, and a Brinell hardness of ≥200HBW.

4. The high manganese steel frog welding repair electrode according to claim 1, characterized in that: The powder is composed of 32-38% marble, 4-7% fluorite, 2-3% silicon powder, 30-40% metallic manganese, 3-6% rutile, 0.5-1% soda ash, 6-8% chromium powder, 2-3% molybdenum powder, 3-4.5% nickel powder, 1-3% graphite and 1-2% roasted mica by mass percentage.

5. A welding method using the high manganese steel frog welding repair electrode according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) no preheating before welding, and the interpass temperature is 90-100° C.; 2) arc welding is adopted, the welding current is 120A-160A, and the welding speed is 2.5-5.5mm / s.

Citation Information

Patent Citations

  • Wear resistant and anti-fatigue surfacing electrode

    CN101274395A

  • Electric welding rod for high-manganese austenite low-temperature steel

    CN108971795A

  • Welding electrode for repair-welding of bainite steel turnout and preparation method thereof

    CN109262164A

  • Welding electrode for high manganese steel turnout repair welding and preparation method for welding electrode

    CN109317863A

  • Electrode for welding high alloy steels

    EP0767029A1