Welding seam cleaning method and filling method for spliced target blank

By heating the blade to a specific temperature, the excess jelly material of the target weld is vertically cleaned and the gaps in the weld are filled in parallel, solving the problems of cleaning and filling in the prior art, and achieving efficient and low-cost weld treatment , improves the quality and operational convenience of the target material.

CN118926823APending Publication Date: 2024-11-12XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125833.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has difficulties in cleaning and filling the target welds, especially since indium is a soft metal, the cleaning process is laborious and inconvenient to fill, and the alternating use of common tools is troublesome, making it difficult to effectively solve the problem of excess solder and gaps in the welds.

Method used

Use a tool that heats the blade to a specific temperature to clean the excess solder perpendicular to the back plate, and pushes the matching indium wire in a parallel manner to the back plate for repair welding. The softening state of the indium wire can be used to achieve cleaning and filling. The same tool can be used to Cleaning and filling, it is highly versatile and low cost.

Benefits of technology

By heating the blade to a temperature of 160-180℃, the solder is cleaned vertically and the weld is filled in parallel with the temperature of 160-165℃, the excess solder and welding notches are easily cleaned, and efficiency and safety are improved, and the tool avoids targeting. The scratches reduce operational difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926823A_ABST
    Figure CN118926823A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of target material production, and discloses a welding seam cleaning method and filling method for a spliced target blank. According to the cleaning method, a blade is heated to a first preset temperature, the blade kept at the first preset temperature is adopted to clean welding flux in the mode of being perpendicular to a back plate, and indium blocks are softened, so that the welding seam is formed; redundant solder located on the periphery of the target blank and in gaps can be easily cleaned; according to the filling method, the blade is heated to the second preset temperature, the blade kept at the second preset temperature is adopted to push the indium wire matched with the notch in size into the notch according to the notch position of the weld joint on the periphery of the target blank in the mode of being parallel to the back plate, and repair welding is achieved in the mode of softening the indium wire. And the cleaning method and the filling method adopt the same cutter, so that the universality is high, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target material weld seam processing, and in particular to a weld seam cleaning method and a weld seam filling method for spliced ​​target blanks. Background Art

[0002] Target materials are the target materials bombarded by high-speed energetic particles and are used to prepare various functional thin films. During the sputtering coating process, after the target material is hit by ions, its surface atoms are sputtered and scattered and deposited on the substrate to form an electronic thin film. There are many types of target materials. According to the material, they can be divided into metal targets, ceramic targets, alloy targets, etc.; according to the application field, they can be divided into targets for semiconductors, targets for display panels, targets for solar cells, etc. In addition, targets can also be classified according to their external dimensions, such as cylindrical, rectangular, etc.

[0003] Target bonding refers to the process of welding the target to the back plate or back tube with solder, which mainly adopts three methods: crimping, brazing and conductive glue. Commonly used solders for target bonding include In, Sn, SnZn, bonding glue, etc. These metal or non-metal solders will more or less remain in the bonding weld.

[0004] CN106378493A discloses a surface treatment method and tool for a target material assembly, wherein the surface treatment method comprises: providing a first tool, the first tool comprising a wedge-shaped tool head with a pointed apex angle; providing a second tool, the second tool comprising a conical tool head; providing a target material assembly, the target material assembly comprising a target material, a backing plate and a weld between the target material and the backing plate, wherein solder is formed in the weld; using the wedge-shaped tool head to remove solder overflowing from the weld; and using the conical tool head to remove solder within a preset depth of the weld.

[0005] The above technical solution first uses a wedge-shaped cutter head to remove the solder overflowing the weld, and then uses a conical cutter head to remove the solder located within a preset depth of the weld, so that the appearance of the formed target assembly meets the preset standard. At the same time, it prevents the solder in the weld from continuing to melt and overflow from the weld due to the high temperature process environment during the subsequent sputtering process, thereby improving the yield of the target assembly.

[0006] Moreover, the above technical solution records in the manual that the solder is indium. Since indium is a soft metal with a certain hardness, the cleaning process is difficult and laborious. The above technical solution uses two tools alternately, which is very troublesome. Moreover, target binding requires not only cleaning of the weld, but also filling of defective welds. Summary of the invention

[0007] The purpose of the present invention is to provide a weld cleaning method and a filling method for spliced ​​target blanks, which can solve the problem of difficult weld cleaning and filling. The cleaning method heats a blade to a first preset temperature, uses the blade maintained at the first preset temperature to clean the solder in a manner perpendicular to a back plate, and softens the indium block to easily clean the excess solder located at the periphery of the target blank and in the gap; and the filling method heats a blade to a second preset temperature, uses the blade maintained at the second preset temperature to push an indium wire matching the size of the gap into the gap in a manner parallel to the back plate according to the notch position of the weld at the periphery of the target blank, and softens the indium wire to achieve repair welding. Moreover, the cleaning method and the filling method use the same tool, which has strong versatility and low cost.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A method for cleaning a weld of a spliced ​​target blank, the spliced ​​target blank comprising a backing plate and at least two target blanks welded to the backing plate, a weld being provided between the target blank and the backing plate, and a gap being provided between the target blanks; the method relates to a tool, the tool being provided with a blade, and the tool being provided with a heating device for heating the blade;

[0010] The method is specifically:

[0011] The heating device heats the blade to a first preset temperature; the first preset temperature is higher than the melting point of indium;

[0012] The blade maintained at the first preset temperature is moved perpendicularly to the back plate along the length direction of the weld to clean the excess solder located at the periphery of the target blank and in the gap.

[0013] Among them, the melting point of indium is 156.6℃. Above this temperature, indium will gradually soften or even melt.

[0014] Preferably, the tool comprises an outer shell, one end of the outer shell is provided with a groove, the heating device is located in the groove, and the outer shell is provided with a connecting piece, and the outer shell detachably connects the blade to the heating device through the connecting piece.

[0015] Preferably, a boss is provided in the groove, the heating device is located in the boss, a through groove matching the boss is provided on the blade, the connecting piece includes a stud, a threaded hole matching the stud is provided on the outer shell, a concave cavity matching the boss is provided at the bottom of the stud, and the concave cavity can cooperate with the boss to press the blade.

[0016] Preferably, one end of the outer shell close to the groove is provided with symmetrically arranged arc surfaces, and the side surface of the outer shell is also provided with a display module, and the display module is used to display the temperature of the blade.

[0017] Preferably, the blade is an edgeless blade, and the blade is a square structure, the thickness of the blade is 0.1mm to 0.15mm, and the blade is a stainless steel blade. The blade can be a square blade or a rectangular blade, and the thickness can be 0.1mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, 0.15mm, but it is not limited to the listed values, and other values ​​not listed in this numerical range are applicable.

[0018] Preferably, when cleaning the solder in the gap, the time for the blade to be inserted into the gap once is less than 30 seconds. Because the purpose of the present invention is cleaning, the time for the blade to be inserted into the target blank once should be as long as possible, provided that the time is less than 30 seconds.

[0019] Preferably, the time for the blade to be inserted into the gap once is 25 to 29 seconds, and specifically, 25 seconds, 26 seconds, 27 seconds, 28 seconds, and 29 seconds may be used, but the values ​​listed are not limited thereto, and other values ​​not listed within this numerical range are applicable.

[0020] Preferably, the first preset temperature is 160-180° C. In practice, 160° C., 165° C., 170° C., 175° C., and 180° C. may be used, but are not limited to the listed values, and other values ​​not listed within this numerical range are applicable.

[0021] At the same time, the present invention also discloses a method for filling a weld, the method involves the above-mentioned tool, and the method is specifically as follows:

[0022] The heating device heats the blade to a second preset temperature; the second preset temperature is higher than the melting point of indium;

[0023] According to the notch position of the weld seam at the periphery of the target blank, a blade maintained at a second preset temperature is pushed into the notch in a manner parallel to the back plate to push an indium wire matching the notch size.

[0024] Preferably, the second preset temperature is 160-165° C. In practice, 160° C., 161° C., 162° C., 163° C., 164° C., and 165° C. may be used, but are not limited to the listed values, and other values ​​not listed within this numerical range are applicable.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The cleaning method of the present invention heats the blade to a first preset temperature, uses the blade maintained at the first preset temperature to clean the solder in a manner perpendicular to the back plate, and softens the indium block to easily clean the excess solder located at the periphery of the target blank and in the gap.

[0027] The filling method of the present invention heats a blade to a second preset temperature, and uses the blade maintained at the second preset temperature to push an indium wire matching the size of the gap into the gap in parallel with the back plate according to the gap position of the weld seam on the periphery of the target blank, and achieves repair welding by softening the indium wire. In addition, the cleaning method and the filling method use the same tool, which has strong versatility and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is an exploded view of the tool of Example A1;

[0029] Figure 2 is a front view of the outer housing of the tool of Example A1;

[0030] Figure 3 yes Figure 2 BB cross-sectional view;

[0031] Figure 4 It is one of the target blank crack defect diagrams of the present invention;

[0032] Figure 5 This is the second target blank crack defect diagram of the present invention;

[0033] Figure 6 is a target blank scratch defect diagram of the present invention;

[0034] Figure 7 This is one of the defective images of the solder not being completely cleaned according to the present invention;

[0035] Figure 8 This is the second defective figure of the solder of the present invention that is not completely cleaned;

[0036] Fig. 9 This is a defect diagram of the target blank edge collapse of the present invention;

[0037] Fig.10 is a defect diagram that is not completely filled by the solder of the present invention;

[0038] Fig.11 This is a defect diagram of leakage filled by solder of the present invention.

[0039] Wherein, the reference numerals in the accompanying drawings are as follows:

[0040] The tool 1 ; the blade 11 ; the outer shell 12 ; the through slot 111 ; the groove 121 ; the connecting piece 122 ; the threaded hole 123 ; the arc surface 124 ; the boss 1211 ; the stud 1221 ; and the cavity 1222 . DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Before describing the embodiment of the present scheme, in the embodiment of the present invention, two target blanks are used to form a spliced ​​target blank. The technical scheme disclosed in Chinese patent CN106337167A has recorded the method of binding multiple pieces of spliced ​​target materials, so no further explanation is given in this embodiment. Those skilled in the art can know that the spliced ​​target material is a plurality of target blanks welded on a backing plate.

[0043] It should be noted that the periphery mentioned in the embodiment is the perimeter area of ​​the rectangular structure formed by the two target blanks; and because the area of ​​the rectangular structure is composed of two target blanks, there will be a gap between the two target blanks, and a weld in the gap. The weld mentioned here does not refer to the weld formed by welding the two target blanks, but the weld between the target blank and the back plate.

[0044] As for the filling of the weld, since the gap width of the target blank is limited, the indium wire cannot be pushed into the weld located in the gap. Therefore, the weld in the gap does not need to be filled. The filling is only for the weld located outside the target blank.

[0045] Example A1

[0046] refer to Figures 1 to 3 A tool 1 is provided with a blade 11, and a heating device (not shown in the figure) for heating the blade 11 is provided in the tool 1. The blade 11 can be heated to a first preset temperature or a second preset temperature by the heating device.

[0047] Preferably, the tool 1 comprises an outer shell 12 , one end of which is provided with a groove 121 , the heating device is located in the groove 121 , and the outer shell 12 is provided with a connecting piece 122 , through which the outer shell 12 detachably connects the blade 11 to the heating device.

[0048] The outer shell 12 can prevent the temperature of the temperature blade 11 from being transmitted to the hands of the operator; the blade 11 can be detachably connected to the heating device through the connecting piece 122, which can facilitate the removal and replacement of the blade 11.

[0049] Furthermore, a boss 1211 is provided in the groove 121, the heating device is located in the boss 1211, a through groove 111 matching the boss 1211 is provided on the blade 11, the connecting piece 122 includes a stud 1221, a threaded hole 123 matching the stud 1221 is provided on the outer shell 12, and a concave cavity 1222 matching the boss 1211 is provided at the bottom of the stud 1221, and the concave cavity 1222 can cooperate with the boss 1211 to press the blade 11.

[0050] During installation, the blade 11 is installed on the boss 1211 through the through groove 111, and then the stud 1221 is screwed to make the cavity 1222 at the bottom of the stud 1221 move along the direction of the boss 1211 and plug into the boss 1211, so that the bottom of the stud 1221 is pressed on the blade 11, and the blade 11 is fixed on the boss 1211; similarly, during disassembly, it is only necessary to loosen the stud 1221 to make the cavity 1222 detach from the boss 1211 to remove the blade 11.

[0051] Optionally, one end of the outer shell 12 close to the groove 121 is provided with a symmetrically arranged arc surface 124, and a display module (not shown in the figure) is also provided on the side of the outer shell 12, and the display module is used to display the temperature of the blade 11. The display module is used to display the temperature of the blade 11. In the solution disclosed in Chinese patent CN117532663A, it is recorded that a display screen is provided on the handle, and the display module of this embodiment can also adopt this method.

[0052] Preferably, the blade 11 is an edgeless blade 11 , and the blade 11 is a square structure, the thickness of the blade 11 is 0.1 mm to 0.15 mm, and the blade 11 is a blade 11 made of stainless steel.

[0053] The operator can choose to use a blade 11 with a thickness of 0.1mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, or 0.15mm according to actual conditions. The blade 11 with a square structure can make the end of the blade 11 a plane. When cleaning, the end of the blade 11 can be fitted with the back plate to ensure that the blade 11 is perpendicular to the back plate. Moreover, we found that if a tool 1 such as a utility knife is used to clean the solder, since indium is a soft metal and has a certain hardness, it is difficult to control the strength when using the utility knife for cleaning. In addition, the blade 11 of the utility knife is relatively sharp and is easy to scratch the target material, and the service life of the utility knife is also very short. Therefore, the use of a bladeless blade 11 in conjunction with a heating device can not only improve the cleaning effect, but also avoid scratching the target material.

[0054] Example B1

[0055] A method for cleaning the weld of a spliced ​​target blank, in which the tool 1 of embodiment A1 is used, and the thickness of the blade 11 is 0.1 mm;

[0056] The present embodiment is specifically as follows:

[0057] The heating device heats the blade 11 to a first preset temperature; the first preset temperature is 160° C.;

[0058] The blade 11 maintained at the first preset temperature is moved perpendicularly to the back plate along the length direction of the weld to clean the excess solder located at the periphery of the target blank and in the gap.

[0059] The time for the blade 11 to enter the gap once is 25 seconds.

[0060] Example B2

[0061] It is basically the same as Example B1, except that the first preset temperature is 170°C.

[0062] Example B3

[0063] It is basically the same as Example B1, except that the first preset temperature is 180°C.

[0064] Example B4

[0065] It is basically the same as Example B1, except that the first preset temperature is 190°C.

[0066] Example B5

[0067] It is basically the same as the embodiment B1, except that the time for the blade 11 to extend into the gap once is 29 seconds.

[0068] Example B6

[0069] It is basically the same as the embodiment B1, except that the time for the blade 11 to extend into the gap once is 27 seconds.

[0070] Example B7

[0071] It is basically the same as the embodiment B1, except that the time for the blade 11 to extend into the gap once is 35 seconds.

[0072] Example B8

[0073] It is basically the same as the embodiment B1, except that the time for the blade 11 to extend into the gap once is 20 seconds.

[0074] Example C1

[0075] A method for filling a weld, in this embodiment, the tool 1 of embodiment A1 is used, and the thickness of the blade 11 is 0.1 mm;

[0076] The present embodiment is specifically as follows:

[0077] The heating device heats the blade 11 to a second preset temperature; the second preset temperature is 160° C.;

[0078] According to the notch position of the weld seam at the periphery of the target blank, the blade 11 maintained at the second preset temperature is parallel to the back plate to push the indium wire matching the notch size into the notch.

[0079] Example C2

[0080] Basically the same as Example C1, except that the second preset temperature is 165°C.

[0081] Example C3

[0082] Basically the same as Example C1, except that the second preset temperature is 162.5°C.

[0083] Example C4

[0084] Basically the same as Example C1, except that the second preset temperature is 175°C.

[0085] Comparative Example B1

[0086] It is basically the same as Example B1, except that the first preset temperature is 150°C.

[0087] Comparative Example B2

[0088] Basically the same as Example B1, except that the first preset temperature is 156.6°C.

[0089] Comparative Example B3

[0090] The method is basically the same as Example B1, except that a utility knife is used to clean the weld, and the utility knife used is Deli DL018B. The utility knife used does not have a heating function, and the temperature of the blade of the utility knife measured by an infrared thermometer is 21°C.

[0091] Comparative Example B4

[0092] It is basically the same as the embodiment B1, except that when cleaning the weld located at the periphery of the target blank, the blade 11 is parallel to the backing plate.

[0093] Comparative Example B5

[0094] The embodiment is basically the same as the embodiment B1, except that when cleaning the weld seam outside the target blank, the blade 11 is tilted to the backing plate. Since the blade 1 is held by the operator for cleaning, it cannot be kept at a certain tilt angle, which is 10 to 80 degrees.

[0095] Comparative Example C1

[0096] It is basically the same as Example C1, except that the second preset temperature is 150°C.

[0097] Comparative Example C2

[0098] Basically the same as Example C1, except that the second preset temperature is 156.6°C.

[0099] Comparative Example C3

[0100] The embodiment is basically the same as the embodiment C1, except that the blade 11 is perpendicular to the back plate.

[0101] Comparative Example C4

[0102] The embodiment is basically the same as the embodiment C1, except that when filling the weld seam outside the target blank, the blade 11 is tilted to the backing plate. Since the cutter 1 is held by the operator for cleaning, it cannot be kept at a certain tilt angle, which is 10 to 80 degrees.

[0103] The weld seam cleaning methods of spliced ​​target blanks of Examples B1 to B8 and Comparative Examples B1 to B5 were respectively used to clean the weld seam between the target blank and the backing plate, and the specific conditions are shown in Table 1.

[0104] The weld gap between the target material and the backing plate was filled using the weld filling methods of Examples C1 to C4 and Comparative Examples C1 to C4, respectively. The specific details are shown in Table 2.

[0105] Table 1 Cleaning of welds

[0106]

[0107] Table 2 Weld filling situation

[0108]

[0109] Note:

[0110] The test method used in the weld cleaning method of the spliced ​​target blank is as follows: each embodiment and comparative example is tested 20 times, and each time is a complete cleaning of the weld. The results of weld cleaning are as follows:

[0111] A qualified result means that the test reaches an ideal state, takes a short time, is easy to operate, and does not produce any adverse phenomena.

[0112] A good result means that the test barely achieves the desired effect, but there are still some shortcomings, such as being difficult to operate, time-consuming, and prone to undesirable phenomena such as chipping and cracking.

[0113] The result failure means that the test cannot be completed due to abnormal conditions or multiple defects such as chipping and cracking occur during the test.

[0114] The test method used in this weld filling method is: only determine the result of a single filling under the corresponding conditions. For the weld filling method:

[0115] A qualified result means that the test reaches an ideal state, takes a short time, is easy to operate, and does not produce any adverse phenomena.

[0116] A good result means that the test barely achieves the desired effect, but there are still some shortcomings, such as being difficult to operate and time-consuming.

[0117] The result failure is filling failure.

[0118] Result analysis:

[0119] 1. From the results of Examples B1 to B4 and Comparative Examples B1 and B2, it can be seen that when the first preset temperature is 160 to 180°C, the cleaning effect of the weld is most ideal. Because Example B4 uses a temperature greater than 160 to 180°C, but the result is good, it means that too high a temperature will transfer heat to the target blank, causing cracks in the target blank, such as Figure 4 and Figure 5 The results are shown in FIG. 1 ; while the comparative example B1 uses a value lower than the melting point of indium, and the comparative example B2 uses a value of the melting point of indium, and neither exceeds the melting point of indium. Because the blade 11 is exposed to the air and is more in contact with the air, the actual temperature during the cleaning process will be lower than 156.6°C, resulting in excessive cleaning difficulty, causing scratches on the target surface. Figure 6 As shown, the optimal cleaning temperature is in the range of 160 to 180°C.

[0120] 2. From the results of Example B1 and Examples B5 to B8, it can be seen that for cleaning the weld in the gap, because the gap is located between the target blanks, a relatively crowded space is formed, resulting in poor heat dissipation. Therefore, the results of Examples B1, B5, B6, and B8 limited to less than 30 seconds are all qualified, while the result of Example B7 exceeding 30 seconds is good. Figure 4 and Figure 5 As shown, the target blank cracks due to being heated for too long. However, from the perspective of time, the longer the time, the better, provided that the result is satisfactory. Therefore, the result of Example B5 is better than that of Examples B1, B6, and B8.

[0121] 3. From the results of Example B1 and Comparative Example B3, it can be seen that the comparative example B3 uses a utility knife of model Deli DL018B, which does not have a heating function. Even if the same cleaning method is used, it is a hard scraping method. Therefore, the result of comparative example B3 is a failure. The weld cannot be cleaned and scratches appear. The results are as follows Figure 6 , Figure 7 , Figure 8 As shown, and also appeared Fig. 9 In this case, the target blank has chipped corners.

[0122] 4. From the results of Example B1 and Comparative Examples B4 and B5, it can be seen that the results of Comparative Examples B4 and B5 are all failures, indicating that the methods of Comparative Examples B4 and B5 are both unable to clean the weld located at the periphery of the target blank after a long operation, because the tool 1 of Example A1 used is a bladeless blade 11, which can largely avoid scratching the target blank. For the inclined method, it is necessary to adjust the angle multiple times to match the position of the solder, which is not only difficult to clean, but also wastes time. For the horizontal method, the solder will be pushed into the weld more, and it is also necessary to control the depth of the blade 11 to prevent the weld from being cleaned too deeply, which will undoubtedly increase the time, indicating that the method perpendicular to the back plate is the ideal cleaning method.

[0123] 5. From the results of Examples C1 to C4 and Comparative Examples C1 to C2, it can be seen that when the second preset temperature is 160 to 165°C, the filling effect is most ideal, because the indium wire needs to be softened when filling the weld, and the indium wire cannot be completely melted into a liquid state, which will lead to filling failure. Therefore, the results of Examples C1 to C3 are all qualified, and the result of Example C4 is a failure. Fig.10 Fill in the incomplete and Fig.11 As shown in the solder leakage, the temperature used in comparative example C1 is lower than the melting point of indium, and the temperature used in comparative example C2 is the melting point of indium. Both of them do not exceed the melting point of indium, but can also soften the indium wire to a certain extent, so the result is good and the operation time is long.

[0124] 6. From the results of Example C1 and Comparative Examples C3 and C4, it can be seen that the result of Comparative Example C3 is a failure, and the result of Comparative Example C4 is good. This is because the filling work cannot be completed by filling in a manner perpendicular to the back plate, and the blade 11 directly blocks the position of the weld; and although the filling work can be completed by an inclined manner, it is time-consuming, and the blade 11 without an edge cannot push the indium wire into the defective position well. Therefore, the filling method parallel to the back plate is the most ideal method.

[0125] In summary, the cleaning method of the present invention heats the blade to a first preset temperature, and experiments have shown that the first preset temperature is a temperature in the range of 160 to 180°C. The blade maintained at the first preset temperature is used to clean the solder in a manner perpendicular to the back plate, and the excess solder located at the periphery of the target blank and in the gap is easily cleaned by softening the indium block. Moreover, when cleaning the solder in the gap, the time is limited to within 30 seconds, which can protect the target blank from the thermal influence of the tool.

[0126] The filling method of the present invention heats the blade to a second preset temperature. Experiments have shown that the first preset temperature is a temperature in the range of 160 to 165° C. The blade maintained at the second preset temperature is used to push an indium wire matching the size of the gap into the gap in parallel with the back plate according to the gap position of the weld seam on the periphery of the target blank. The indium wire is softened to achieve repair welding. In addition, the cleaning method and the filling method use the same tool, which has strong versatility and low cost.

[0127] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements or modifications without departing from the principle of the present invention. These improvements or modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for cleaning a weld of a spliced ​​target blank, wherein the spliced ​​target blank comprises a backing plate and at least two target blanks welded to the backing plate, a weld is provided between the target blank and the backing plate, and a gap is provided between the target blanks; characterized in that: The method relates to a tool, wherein the tool is provided with a blade, and a heating device for heating the blade is provided inside the tool; The method is specifically as follows: The heating device heats the blade to a first preset temperature; the first preset temperature is higher than the melting point of indium; The blade maintained at the first preset temperature is moved perpendicularly to the back plate along the length direction of the weld to clean the excess solder located at the periphery of the target blank and in the gap.

2. The weld cleaning method of the spliced ​​target blank according to claim 1, characterized in that: The tool comprises an outer shell, one end of which is provided with a groove, the heating device is located in the groove, and the outer shell is provided with a connecting piece, through which the outer shell detachably connects the blade to the heating device.

3. The weld cleaning method of the spliced ​​target blank according to claim 2, characterized in that: A boss is provided in the groove, the heating device is located in the boss, a through groove matching the boss is provided on the blade, the connecting piece includes a stud, a threaded hole matching the stud is provided on the outer shell, a concave cavity matching the boss is provided at the bottom of the stud, and the concave cavity can cooperate with the boss to press the blade.

4. The method for cleaning the weld of a spliced ​​target blank according to claim 2, characterized in that: One end of the outer shell close to the groove is provided with symmetrically arranged arc surfaces, and the side surface of the outer shell is also provided with a display module, and the display module is used to display the temperature of the blade.

5. The method for cleaning the weld of a spliced ​​target blank according to claim 1, characterized in that: The blade is an edgeless blade and has a square structure. The thickness of the blade is 0.1 mm to 0.15 mm. The blade is made of stainless steel.

6. The method for cleaning the weld of a spliced ​​target blank according to claim 1, characterized in that: When cleaning the solder in the gap, the blade is inserted into the gap for less than 30 seconds at a time.

7. The method for cleaning the weld of a spliced ​​target blank according to claim 6, characterized in that: The time for the blade to extend into the gap once is 25 to 29 seconds.

8. The method for cleaning the weld of a spliced ​​target blank according to claim 1, characterized in that: The first preset temperature is 160-180°C.

9. A method for filling a weld, characterized in that: The method relates to the tool according to claim 1, and the method is specifically: The heating device heats the blade to a second preset temperature; the second preset temperature is higher than the melting point of indium; According to the notch position of the weld seam at the periphery of the target blank, the blade maintained at the second preset temperature is parallel to the back plate to push the indium wire matching the notch size into the notch.

10. The method for filling a weld according to claim 9, characterized in that: The second preset temperature is 160-165°C.