Machining method for preventing deformation and out-of-tolerance of finished crankshaft of high-power diesel engine
Through improved crankshaft processing process and equipment, the problem of inaccurate deformation control of high-power diesel engine crankshafts in domestic production is solved, high-precision coaxiality and fatigue resistance are achieved, large-scale production needs are met, and costs are reduced .
Patent Information
- Application Number
- CN202410853629.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-12
AI Technical Summary
In the domestic small batch trial production of high-power diesel engine crankshafts, the medium-frequency induction hardening and processing deformation control are not accurate enough, which makes it difficult to ensure the coaxiality of finishing processing, which limits the improvement of yield and the realization of mass production.
Adopt improved processing processes, including vertical quenching, multiple high-temperature aging treatment, adjusting induction hardening methods and fine grinding processes, increasing low-temperature aging treatment, optimizing the processing equipment and processes of the crankshaft, ensuring the coaxiality and fatigue resistance of the crankshaft performance.
The deformation of the crankshaft is effectively controlled, the coaxiality is within φ0.05mm, the fatigue resistance is improved, the batch production needs of domestic finished crankshafts are met, and the dependence on imported finished products is reduced.
Smart Images

Figure CN118926850A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diesel engine production and processing, and in particular relates to a processing method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine. Background Art
[0002] The crankshaft of a high-power diesel engine is relatively long in total length and consists of multiple main journals and connecting rod journals. The material is 34CrNiMo6, which has extremely high toughness and high viscosity. It is a typical difficult-to-process material and its design structure is a large aspect ratio and weak rigidity structure. Among them, the finished crankshaft requires the journal and fillet parts to be strengthened by medium-frequency induction quenching. The highest dimensional accuracy is required to reach IT6 level, the coaxiality of the main journal is ≤φ0.05mm, and the coaxiality distribution is not allowed to have sudden changes, such as Figure 1 The figure shows the process design requirements for common finished crankshafts. At present, the processing process of this type of high-power diesel engine crankshaft is: die forging blank → horizontal tempering treatment → correction → rough machining → high temperature aging → fine milling of crankshaft → first low temperature aging → semi-fine grinding of journal and hole system processing → second low temperature aging → induction quenching → fine grinding of journal → inspection. According to the above original crankshaft processing procedures, the following problems were found in the early research and development process: when the crankshaft was finely processed to the finished product, although the full process technology state of crankshaft forging, heat treatment strengthening and mechanical processing was initially realized, the technical indicators of the sample met the product design requirements. However, in the process of small-scale trial production of this type of high-power diesel engine crankshaft in the localization, problems such as inaccurate control of medium-frequency induction quenching and processing deformation, and difficulty in ensuring the coaxiality of fine processing were exposed, which restricted the further improvement of the yield rate, and there was still a certain gap to meet the mass production of finished crankshafts for domestic high-power diesel engines. Summary of the invention
[0003] In view of this, the invention aims to overcome the defects in the prior art and proposes a processing method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine.
[0004] To achieve the above object, the technical solution created by the present invention is implemented as follows:
[0005] A method for processing a finished crankshaft of a high-power diesel engine to prevent deformation and out-of-tolerance, comprising the following steps:
[0006] S1. Vertical quenching and tempering treatment: Place the crankshaft vertically into the heating furnace so that the entire cross section of the crankshaft is heated evenly;
[0007] S2, Rough machining: Rough milling of crankshaft main journal and connecting rod journal;
[0008] S3, first high temperature aging: high temperature aging treatment of the crankshaft;
[0009] S4, fine milling of crankshaft: fine milling of crankshaft main journal and connecting rod journal;
[0010] S5, second high temperature aging: the crankshaft after fine milling is subjected to a second high temperature aging treatment;
[0011] S6, machining: semi-finishing grinding of journal and hole system;
[0012] S7, the third high temperature aging: the crankshaft after semi-finished grinding of the journal and hole system is subjected to the third high temperature aging treatment;
[0013] S8, Induction hardening: Use special induction hardening tooling to induction harden the crankshaft;
[0014] S9, hole system processing: processing the crankshaft oil plugging hole and inclined oil hole;
[0015] S10, first fine grinding of the main journal and connecting rod journal, followed by low temperature aging;
[0016] S11. Second fine grinding of main journal and connecting rod journal: The main journal and connecting rod journal are finely ground twice more and inspected. The finished crankshaft is then processed.
[0017] Furthermore, the coaxiality of the finished crankshaft is within φ0.05mm.
[0018] Further, the crankshaft is placed vertically into a pit-type heating furnace.
[0019] Furthermore, in step S6, when semi-finishing the journal and the hole system, the main journal is ground first, then the connecting rod journal is ground, and finally the hole system is processed.
[0020] Furthermore, the hole system processing includes drilling spindle oil channel holes, inclined oil holes, and oil plugging holes.
[0021] Furthermore, a low-temperature aging treatment is added between the two fine grinding processes.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] The present invention controls the deformation of a finished crankshaft of a high-power diesel engine by improving the finished crankshaft processing flow, changing the crankshaft processing equipment, etc., thereby ensuring its coaxiality, improving its fatigue resistance, meeting the mass production of domestic finished crankshafts, reducing the demand for imports of finished crankshafts of this model, and reducing factory cost expenditure. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments and descriptions of the present invention are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:
[0025] Figure 1This is a schematic diagram of a finished crankshaft processed by the present invention. DETAILED DESCRIPTION
[0026] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0027] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0028] In the description of the invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.
[0029] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0030] A method for processing a finished crankshaft of a high-power diesel engine to prevent deformation and out-of-tolerance, comprising the following steps:
[0031] S1. Vertical quenching and tempering treatment: Place the crankshaft vertically into a pit-type heating furnace so that the entire cross section of the crankshaft is heated evenly.
[0032] S2, Rough machining: Rough milling of crankshaft main journal and connecting rod journal;
[0033] S3, first high temperature aging: high temperature aging treatment of the crankshaft;
[0034] S4, fine milling of crankshaft: fine milling of crankshaft main journal and connecting rod journal;
[0035] S5, second high temperature aging: the crankshaft after fine milling is subjected to a second high temperature aging treatment;
[0036] S6. Machining: semi-finishing grinding of journals and hole system processing; when semi-finishing grinding of journals and hole system processing, first grind the main journal, then grind the connecting rod journal, and finally perform hole system processing; hole system processing includes drilling the main shaft oil channel hole, inclined oil hole, and oil plug hole.
[0037] S7, the third high temperature aging: the crankshaft after semi-finished grinding of the journal and hole system is subjected to the third high temperature aging treatment;
[0038] S8, Induction hardening: Use special induction hardening tooling to induction harden the crankshaft;
[0039] S9, hole system processing: processing the crankshaft oil plugging hole and inclined oil hole;
[0040] S10, first fine grinding of the main journal and connecting rod journal, followed by low temperature aging;
[0041] S11. Second fine grinding of main journal and connecting rod journal: The main journal and connecting rod journal are finely ground twice again, and a low temperature aging treatment is added between the two fine grinding processes. Then the finished crankshaft is inspected and the finished crankshaft is processed. The coaxiality of the finished crankshaft can be controlled within φ0.05mm.
[0042] The present invention optimizes and improves the prior art of "horizontal quenching and tempering treatment → correction → rough machining → high temperature aging → fine milling of crankshaft → first low temperature aging → semi-fine grinding of journal and hole system processing → second low temperature aging → induction quenching → fine grinding of journal → inspection" into "vertical quenching and tempering treatment → rough machining → first high temperature aging → fine milling of crankshaft → second high temperature aging → semi-fine grinding of journal and hole system processing → third high temperature aging → induction quenching → hole system processing → first fine grinding of main journal and connecting rod journal → low temperature aging → second fine grinding of main journal and connecting rod journal → inspection".
[0043] In the prior art, a horizontal heating furnace is used for quenching and tempering. During the heating process, the crankshaft is bent due to its own weight. During quenching, the crankshaft is horizontally immersed in the quenching liquid. The cooling speed of the upper and lower cross sections is different, which destroys the structural deformation of the crankshaft. In this solution, in order to better control the deformation of the crankshaft during quenching and tempering, the horizontal heating furnace is changed to a pit-type heating furnace, which effectively eliminates the influence of the crankshaft's own weight on the deformation. During quenching, the crankshaft is vertically immersed in the quenching liquid, and the entire cross section of the crankshaft is heated evenly, reducing the bending deformation caused by quenching.
[0044] In the prior art, the crankshaft after fine milling is subjected to the first low temperature aging treatment, and the low temperature aging treatment is generally used for workpieces after fine grinding. High temperature aging treatment is more effective in reducing the internal residual stress of the workpiece for casting, forging, welding blanks and workpieces after rough machining. Therefore, in this scheme, in order to better control the deformation of the crankshaft during machining, the first low temperature aging is changed to the second high temperature aging, which effectively eliminates the residual stress inside the crankshaft after fine milling.
[0045] In the prior art, during the semi-finished grinding of the journal and the hole system, three types of hole systems, namely, the spindle oil channel hole, the oblique oil hole, and the oil plug hole, must be processed. However, practical research has shown that during the subsequent induction quenching, the oil plug hole and the oblique oil hole structure affect the diffusion of the local heat of the connecting rod journal deformation unit, making the part of the crank arm close to the oil plug hole prone to overburning, and also increasing the risk of cracking; the thin structure of the inclined surface of the crank arm causes uneven heating of the journal circumference at this part, resulting in increased deformation of the connecting rod journal. Therefore, in order to reduce deformation, in this process scheme, only the spindle oil channel hole is processed during the semi-finished grinding of the journal and the hole system.
[0046] In the prior art, the crankshaft undergoes a second low-temperature aging treatment after fine milling, and the low-temperature aging treatment is generally used for workpieces after fine grinding. High-temperature aging treatment is more effective in reducing the internal residual stress of the workpiece for cast, forged, welded blanks and workpieces after rough machining. In this solution, in order to better control the deformation of the crankshaft during machining, the second low-temperature aging is changed to the third high-temperature aging, which effectively eliminates the internal residual stress of the crankshaft after fine milling. At the same time, compared with the second high-temperature aging treatment, the internal stress of the crankshaft is further stabilized.
[0047] In the prior art, during the induction quenching of the crankshaft, the main journal is quenched first and then the connecting rod journal. However, practical studies have shown that during the induction quenching process, the deformation of the connecting rod journal is greater than that of the main journal, and the deformation directions of the two are opposite. In order to offset the deformation of the connecting rod journal and the main journal and achieve the purpose of reducing the overall deformation, in this scheme, during the induction quenching process, the connecting rod journal is quenched first and then the main journal, and the quenching of the connecting rod journal and the main journal is carried out in a "symmetrical from the middle to both sides" manner.
[0048] In this scheme, the processing steps for the crankshaft oil plugging holes and inclined oil holes are added. In order to reduce the deformation of the crankshaft during the processing, the oil plugging holes and the inclined oil holes are processed after induction quenching, thereby avoiding the problem of increased deformation of the crankshaft due to the incomplete metal material on the inclined surface of the crank arm during the induction quenching process.
[0049] In the prior art, the main journal and connecting rod journal are finely ground once, because after the induction hardening process, the crankshaft re-forms a high residual stress inside. When the grinding process is carried out, it will be accompanied by a strong release of internal stress, resulting in large deformation. The coaxiality of the crankshaft after fine grinding is not easy to guarantee, generally between φ0.08-φ0.10mm. In this scheme, a low-temperature aging treatment and a fine grinding process of the main journal and connecting rod journal are added. After the first fine grinding of the main journal and connecting rod journal, new residual stress is generated inside the crankshaft. A low-temperature aging treatment is performed to eliminate the residual stress generated inside the crankshaft, and then the main journal and connecting rod journal are finely ground to size for the second time, which alleviates the large deformation of the crankshaft caused by the strong internal stress released during the fine grinding process. After measurement, the coaxiality is within φ0.05mm, which meets the crankshaft process requirements.
[0050] During the second fine grinding, the main journal and connecting rod journal are fine ground twice, and a low-temperature aging treatment is added. After the crankshaft has been fine ground for the first time, new residual stress is generated inside the crankshaft. A low-temperature aging treatment is performed to eliminate the residual stress generated inside the crankshaft, and then the main journal and connecting rod journal are fine ground for the second time to size, thereby avoiding the crankshaft from being deformed significantly due to the strong internal stress released during the fine grinding process.
[0051] The present invention effectively eliminates the internal residual stress of the crankshaft during the machining process by changing the tempering treatment method, adjusting the number of high-temperature aging treatments, adjusting the processing procedures of the inclined oil holes and the oil plugging holes, adjusting the induction quenching method, and fine grinding the main journal and the connecting rod journal twice during the crankshaft machining process. After the third high-temperature aging treatment, the runout values of each crankshaft journal are all less than 0.3mm; after two fine grindings of the main journal and the connecting rod journal, the coaxiality of the crankshaft is guaranteed. After measurement, the coaxiality of the crankshaft can be controlled within φ0.05mm, which meets the process requirements, improves its fatigue resistance, meets the mass production needs of domestic finished crankshafts, and provides technical guidance for the machining and manufacturing of finished crankshafts of the same type.
[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preventing deformation and out-of-tolerance of finished crankshafts of high-power diesel engines, characterized in that: The steps include: S1. Vertical quenching and tempering treatment: Place the crankshaft vertically into the heating furnace so that the entire cross section of the crankshaft is heated evenly; S2, Rough machining: Rough milling of crankshaft main journal and connecting rod journal; S3, first high temperature aging: high temperature aging treatment of the crankshaft; S4, fine milling of crankshaft: fine milling of crankshaft main journal and connecting rod journal; S5, second high temperature aging: the crankshaft after fine milling is subjected to a second high temperature aging treatment; S6, machining: semi-finishing grinding of journal and hole system; S7, the third high temperature aging: the crankshaft after semi-finished grinding of the journal and hole system is subjected to the third high temperature aging treatment; S8, Induction hardening: Use special induction hardening tooling to induction harden the crankshaft; S9, hole system processing: processing the crankshaft oil plugging hole and inclined oil hole; S10, first fine grinding of the main journal and connecting rod journal, followed by low temperature aging; S11. Second fine grinding of main journal and connecting rod journal: The main journal and connecting rod journal are finely ground twice more and inspected. The finished crankshaft is then processed.
2. The method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine according to claim 1 is characterized in that: The coaxiality of the finished crankshaft is within φ0.05mm.
3. The method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine according to claim 1 is characterized in that: In step S1, the crankshaft is placed in a pit-type heating furnace.
4. The method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine according to claim 1 is characterized in that: In step S6, when semi-finishing the journal and the hole system, the main journal is ground first, then the connecting rod journal is ground, and finally the hole system is processed.
5. A method for preventing deformation and out-of-tolerance processing of a finished crankshaft of a high-power diesel engine according to claim 4, characterized in that: In step S6, the hole system processing includes drilling the spindle oil channel hole, the inclined oil hole, and the oil plugging hole.
6. The method for preventing deformation and out-of-tolerance of a finished crankshaft of a high-power diesel engine according to claim 1, characterized in that: In step S11, a low-temperature aging treatment is added between the two fine grinding processes.
Citation Information
Patent Citations
Processing process of automobile engine crank shaft
CN104384874A
Heat treatment deformation control method for medium-frequency quenching of high-power crankshaft
CN113969334A
Heat treatment method for high-bearing slender hollow crankshaft
CN117512317A
Diesel engine crankshaft quenching method for controlling deformation
CN117587199A
Crank shaft having high fatigue strength and its production method
JP2008127620A
Cited By
Method for machining camshaft with high hardness and large length-diameter ratio
CN121199573A