Grinding and polishing integrated composite grinding tool and preparation method and application thereof
Through integrated composite abrasive tools, combined with consolidation and free abrasive technology, the problems of low processing efficiency and surface scratches are solved, and high-efficiency and low-pollution grinding and polishing effects are achieved, and the surface quality of the workpiece is improved.
Patent Information
- Application Number
- CN202411315414.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-19
AI Technical Summary
In the prior art, the free abrasive particles have low processing efficiency, poor uniformity within the sheet, low abrasive utilization rate, large waste liquid pollution, and the surface of the workpiece with consolidated abrasive particles polishing technology is severely scratched, and it is necessary to cooperate with the free abrasive particles fine-polishing treatment.
Adopt integrated composite abrasive tools, including a base layer and abrasive layer, the first abrasive and organic composite microsphere pore-making agent are consolidated in the abrasive layer. The hardness of the second abrasive is ≤ the hardness of the first abrasive, and is bonded through water-soluble bonding. The agent forms an open hole structure, improves the chip space of the abrasive tool, reduces scratches, and realizes integrated processing of grinding and polishing.
Improve processing efficiency and workpiece surface quality, reduce scratches and waste liquid pollution, avoid further polishing, and achieve high-efficiency grinding and polishing.
Smart Images

Figure CN118927171A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of grinding and polishing processing, and in particular to a grinding and polishing integrated composite abrasive tool and a preparation method and application thereof. Background Art
[0002] Sapphire, ceramics, glass, silicon wafers and other hard and brittle materials have played an important role in many fields such as electronic information, military industry, aerospace, etc. due to their unique high strength, high hardness, corrosion resistance, high temperature resistance, wear resistance and other excellent properties. Due to the development of cutting-edge technologies in aerospace, electronic information and other fields, higher requirements are placed on the processing efficiency and surface quality of difficult-to-process materials such as silicon carbide, sapphire, ceramics, special glass, etc.
[0003] At present, the polishing of the above materials generally adopts free abrasive processing technology. By using abrasive polishing liquid and elastic polishing pad together, good workpiece surface quality can be obtained. However, the polishing process has the following problems: (1) The grinding tool has no constraints on the movement of the abrasive particles. The randomness of the distribution and movement of the abrasive particles will reduce the processing efficiency and the uniformity within the wafer; (2) The abrasive stays on the surface of the grinding tool for a short time, resulting in low abrasive utilization and large waste liquid pollution.
[0004] At present, some existing technologies use fixed abrasive polishing technology to improve the above problems. By fixing the abrasive in the mold to achieve fully constrained movement of the abrasive, the uniformity of abrasive distribution, material removal efficiency and abrasive utilization can be improved. However, due to processing defects such as surface damage and scratches caused by abrasive plowing under the two-body wear mechanism, this technology still cannot completely replace the traditional free polishing technology. The fixed abrasive polishing process still needs to be combined with the free abrasive fine polishing process. Based on the above background, it is of great significance to develop an efficient and precise processing technology that takes into account both processing efficiency and polishing quality.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide an integrated grinding and polishing composite abrasive tool to solve the technical problems in the prior art, such as low processing efficiency, poor uniformity within the sheet, low abrasive utilization rate, and large waste liquid pollution of free abrasive processing technology, as well as serious scratches on the workpiece surface of fixed abrasive polishing technology, and the need for free abrasive fine polishing after fixed abrasive polishing. The integrated grinding and polishing composite abrasive tool provided by the present invention can simultaneously realize integrated grinding and polishing processing, with few scratches, good surface quality, and high material removal rate, taking into account both high processing efficiency and good workpiece surface quality.
[0007] The second object of the present invention is to provide a method for preparing the integrated grinding and polishing composite abrasive tool as described above.
[0008] The third object of the present invention is to provide a method for grinding and polishing a workpiece, wherein the workpiece is ground and polished using the above-mentioned integrated grinding and polishing composite abrasive tool.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] A grinding and polishing integrated composite abrasive tool comprises a base layer and an abrasive layer, wherein a first abrasive and an organic composite microsphere pore-forming agent are solidified in the abrasive layer, wherein the organic composite microsphere pore-forming agent is a spherical or nearly spherical composite comprising a second abrasive and a water-soluble adhesive, and the hardness of the second abrasive is ≤ the hardness of the first abrasive.
[0011] Preferably, in terms of mass percentage, the abrasive layer comprises 30%-60% of a resin binder, 3%-20% of the first abrasive, 3%-35% of the organic composite microsphere pore-forming agent, 3%-10% of a filler and 0.2%-15% of an additive.
[0012] Preferably, the particle size of the organic composite microsphere pore-forming agent is 20-90 μm.
[0013] Preferably, in the organic composite microsphere pore-forming agent, the mass percentage of the water-soluble adhesive is 2.5%-10%.
[0014] Preferably, the preparation method of the organic composite microsphere pore-forming agent is one of centrifugal spray granulation, rolling granulation or inverse microemulsion polymerization.
[0015] Preferably, the water-soluble adhesive includes at least one of cyclodextrin, dextrin, starch, hydroxymethyl cellulose, methyl cellulose, polyacrylic acid, polyacrylamide and polyvinyl alcohol.
[0016] Preferably, the second abrasive includes at least one of aluminum oxide, silicon dioxide and cerium oxide.
[0017] Preferably, the Mohs hardness of the second abrasive is 6-9.
[0018] Preferably, the particle size of the second abrasive is 100-500 nm.
[0019] Preferably, the first abrasive includes at least one of diamond, silicon carbide, cubic boron nitride, zirconium oxide and corundum.
[0020] Preferably, the first abrasive has a Mohs hardness of 7-10.
[0021] Preferably, the particle size of the first abrasive is 20-500 nm.
[0022] Preferably, the median particle size of the second abrasive is not less than the median particle size of the first abrasive.
[0023] Preferably, the resin binder includes at least one of unsaturated polyester, epoxy resin and polyurethane.
[0024] Preferably, the filler includes one or more combinations of graphite, carbon black, carbon fiber staple fibers, carbon nanotubes, calcium carbonate, and calcium silicate.
[0025] Preferably, the auxiliary agent includes at least one of an initiator, a curing agent and a dispersant.
[0026] A method for preparing the above-mentioned integrated grinding and polishing composite abrasive tool comprises the following steps:
[0027] S1. The raw materials of the abrasive layer are mixed and degassed to obtain a mixture, and the mixture is placed in a molding mold;
[0028] S2. A base layer is applied to the non-grinding and polishing surface of the mixture, and the grinding and polishing integrated composite abrasive tool is obtained through solidification; or, the mixture is first solidified to obtain an abrasive layer, and then the base layer is adhered to the non-grinding and polishing surface of the abrasive layer to obtain the grinding and polishing integrated composite abrasive tool.
[0029] A method for grinding and polishing a workpiece, comprising grinding and polishing the workpiece using the above-mentioned integrated grinding and polishing composite abrasive tool.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The integrated grinding and polishing composite abrasive provided by the present invention has a first abrasive and an organic composite microsphere pore-forming agent fixed in the abrasive layer. During the process of machining a workpiece, the first abrasive acts as a fixed abrasive to grind the workpiece and improve the material removal rate. During the process of machining a workpiece, the organic composite microsphere pore-forming agent on the surface layer meets the water-based grinding fluid on the surface of the abrasive tool, and the water-soluble adhesive is physically dissolved to form an open pore structure on the surface of the abrasive tool. The pore structure contains a freely distributed second abrasive. On the one hand, the organic composite microsphere pore-forming agent acts as a pore-forming agent to increase the chip holding space inside the abrasive tool and reduce the hardness of the abrasive tool matrix, thereby reducing scratches on the workpiece surface and enhancing the self-sharpening property of the abrasive tool. On the other hand, the free abrasive component is introduced into the composite abrasive tool to polish the workpiece and improve the surface quality of the material. The integrated grinding and polishing process can be realized simultaneously, with few scratches, good surface quality, and high material removal rate, taking into account both high machining efficiency and good workpiece surface quality.
[0032] (2) The integrated grinding and polishing composite abrasive tool provided by the present invention is used to grind and polish the surface of the workpiece. Compared with the traditional free abrasive polishing technology, the abrasive consumption is small and the waste liquid pollution can be reduced; compared with the traditional fixed abrasive processing technology, the processed workpiece has fewer scratches and better surface quality, and no further fine polishing treatment is required. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 A schematic diagram of the preparation process of the organic composite microsphere pore-forming agent provided in an embodiment of the present invention;
[0035] Figure 2 A schematic diagram of a forming process of a grinding and polishing integrated composite abrasive tool provided in an embodiment of the present invention;
[0036] Figure 3 A schematic diagram of the working surface of the integrated grinding and polishing composite abrasive tool provided in an embodiment of the present invention;
[0037] Figure 4 A diagram of the grinding mechanism of the integrated grinding and polishing composite abrasive tool provided in an embodiment of the present invention;
[0038] Figure 5 Surface morphology of the integrated grinding and polishing composite abrasive tool provided by an embodiment of the present invention (wherein the leftmost picture is the overall surface picture of the composite abrasive tool, the middle picture is the holes formed on the surface of the composite abrasive tool by the organic composite microsphere pore-forming agent, and the rightmost picture is the second abrasive in a free state in the hole);
[0039] Figure 6 A schematic diagram of the working process of the grinding and polishing device provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0040] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0041] The first aspect of the present invention provides an integrated grinding and polishing composite abrasive tool, comprising a base layer and an abrasive layer, wherein a first abrasive and an organic composite microsphere pore-forming agent are solidified in the abrasive layer, and the organic composite microsphere pore-forming agent is a spherical or nearly spherical composite comprising a second abrasive and a water-soluble adhesive, and the hardness of the second abrasive is ≤ the hardness of the first abrasive.
[0042] In view of the problems in the prior art of low processing efficiency, poor uniformity within the sheet, low abrasive utilization rate, large waste liquid pollution in free abrasive processing technology and serious scratches on the workpiece surface in fixed abrasive processing technology, the present invention provides an integrated grinding and polishing composite abrasive tool, which combines the advantages of fixed abrasive processing and free abrasive processing, can simultaneously realize integrated grinding and polishing processing, has few scratches, good surface quality, high material removal rate, and takes into account both high processing efficiency and good workpiece surface quality.
[0043] In the present invention, a first abrasive and an organic composite microsphere pore-forming agent are fixed in the abrasive layer. Figure 3 and Figure 5 As shown, the first abrasive acts as a fixed abrasive to grind the workpiece and improve the material removal rate; the organic composite microsphere pore-forming agent on the surface of the composite abrasive tool contacts the water-based grinding fluid on the surface of the abrasive tool during the workpiece processing, and the water-soluble adhesive dissolves to form an open pore structure on the surface of the abrasive tool. The pore structure contains the second abrasive distributed freely. The organic composite microsphere pore-forming agent acts as a pore-forming agent to increase the chip space inside the abrasive tool and reduce the hardness of the abrasive tool matrix, thereby reducing scratches on the workpiece surface and enhancing the self-sharpening of the abrasive tool. On the other hand, the free abrasive component is released in situ during the working process of the composite abrasive tool to polish the workpiece and improve the surface quality of the material; thereby realizing the integrated processing of grinding and polishing.
[0044] The hardness of the first abrasive is controlled to be not less than that of the second abrasive. The first abrasive with relatively high hardness is selected as the fixed abrasive for grinding, and the second abrasive with relatively low hardness is selected as the free abrasive for polishing, which can ensure both high grinding efficiency and surface quality of the workpiece.
[0045] In some specific embodiments of the present invention, the first abrasive and the organic composite microsphere pore former are uniformly distributed in the abrasive layer.
[0046] In some specific embodiments of the present invention, the abrasive layer includes, by mass percentage, 30%-60% of resin binder, 3%-20% of first abrasive, 3%-35% of organic composite microsphere pore former, 3%-10% of filler and 0.2%-15% of additive.
[0047] Among them, the resin binder plays the role of fixing the first abrasive, organic composite microsphere pore-forming agent, filler and other components. It is the key part of the composite abrasive tool to bear and transfer loads and maintain the polishing liquid environment; the filler plays the role of enhancing the strength of the grinding layer, and the additive mainly plays the role of initiating the reaction or increasing the cross-linking degree of the resin system or promoting the dispersion of components.
[0048] In some embodiments, typically but not limiting, for example, the mass percentage of the resin binder in the abrasive layer can be any value among 30%, 35%, 39%, 45%, 52%, 55%, 60%, or a range of values consisting of any two values; the mass percentage of the first abrasive can be any value among 3%, 5%, 8%, 11%, 15%, 18%, 20%, or a range of values consisting of any two values; the mass percentage of the organic composite microsphere pore-forming agent can be 3%, 5%, 10%, 15%, 20%, 25%, .... The mass percentage of the filler can be any point value among 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range value composed of any two point values; the mass percentage of the auxiliary agent can be any point value among 0.2%, 0.5%, 1%, 1.5%, 2%, 3%, 5%, 8%, 10%, 12%, 15% or a range value composed of any two point values.
[0049] In some specific embodiments of the present invention, the particle size of the organic composite microsphere pore former is 20-90 μm, for example, it can be any point value among 20 μm, 25 μm, 32 μm, 38 μm, 45 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or a range value composed of any two point values; if the particle size of the organic composite microsphere pore former is too small, the screening equipment cannot accurately screen and control the particle size of the pore former during preparation, and the diameter of the open holes formed on the surface of the abrasive tool during the processing of the workpiece is too small, and the effect of polishing the workpiece, improving the surface quality of the material and enhancing the self-sharpening of the abrasive tool is not good; if the particle size of the organic microsphere pore former is too large, the structural stability of the polishing surface of the abrasive tool is easily destroyed, and the stability of the polishing effect cannot be guaranteed; therefore, it is necessary to reasonably control the particle size range of the organic composite microsphere pore former.
[0050] In some specific embodiments of the present invention, in the organic composite microsphere pore-forming agent, the mass percentage of the water-soluble adhesive is 2.5%-10%, for example, it can be any point value among 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range value consisting of any two point values.
[0051] If the content of water-soluble adhesive in the organic composite microsphere pore-forming agent is too low, the second abrasive may become loose and difficult to bond and aggregate into balls. If the content of water-soluble adhesive is too high, the content of the second abrasive in the organic composite microsphere pore-forming agent may be too low, which may lead to too low content of the second abrasive in the open pores of the composite abrasive tool and poor polishing effect of the free abrasive. Therefore, it is necessary to reasonably control the composition and content of the organic composite microsphere pore-forming agent.
[0052] like Figure 1 As shown, in some specific embodiments of the present invention, the preparation method of the organic composite microsphere pore-forming agent is a centrifugal spray granulation method, comprising the following steps:
[0053] The second abrasive, a water-soluble adhesive and water are mixed and dispersed to obtain a water dispersion with a mass fraction of the second abrasive of 10%-35%, and the water dispersion is granulated and screened by using a centrifugal spray granulation technology to obtain the product.
[0054] In some specific embodiments of the present invention, when preparing the aqueous dispersion, the mixing and dispersing method includes shearing dispersion and / or ultrasonic dispersion.
[0055] In some specific embodiments of the present invention, granulation is carried out in a centrifugal spray drying device, the inlet speed of the aqueous dispersion is 10-40 ml / min, the inlet air temperature is 160-250° C., and the centrifugal frequency is 200-400 Hz.
[0056] In some embodiments, typically but not limiting, for example, the mass fraction of the second abrasive in the aqueous dispersion can be any value among 10%, 15%, 20%, 25%, 30%, 35%, or a range consisting of any two values; the liquid inlet speed of the aqueous dispersion can be any value among 10 ml / min, 20 ml / min, 30 ml / min, 40 ml / min, or a range consisting of any two values; the air inlet temperature can be any value among 160°C, 180°C, 200°C, 210°C, 230°C, 250°C, or a range consisting of any two values; the centrifugal frequency can be any value among 200 Hz, 220 Hz, 250 Hz, 280 Hz, 300 Hz, 320 Hz, 350 Hz, 380 Hz, 400 Hz, or a range consisting of any two values.
[0057] Too high (or too low) concentration of the aqueous dispersion, too high (or too low) liquid inlet speed, or too low (or too high) centrifugal frequency will cause the particle size of the organic composite microsphere pore-forming agent to be too large (or too small); if the inlet air temperature is too low, the organic composite microsphere pore-forming agent cannot be completely dried and the particles are prone to sticking together and forming lumps; if the inlet air temperature is too high, the water-soluble adhesive may decompose due to heat and the water may dry too quickly, causing the microspheres to break and the shape of the pore-forming agent to be destroyed.
[0058] In other embodiments of the present invention, the organic composite microsphere pore-forming agent can also be prepared by other methods such as a pelletizing method or an inverse microemulsion polymerization method.
[0059] In some specific embodiments of the present invention, the water-soluble adhesive includes at least one of cyclodextrin, dextrin, starch, hydroxymethyl cellulose, methyl cellulose, polyacrylic acid, polyacrylamide, and polyvinyl alcohol; the water-soluble adhesive serves to bond the second abrasive during the preparation of the organic composite microsphere pore-forming agent and the composite abrasive tool.
[0060] In some specific embodiments of the present invention, the second abrasive includes at least one of aluminum oxide, silicon dioxide, and cerium oxide.
[0061] In some specific embodiments of the present invention, the Mohs hardness of the second abrasive is 6-9, for example, 6, 7, 8 or 9.
[0062] In some specific embodiments of the present invention, the particle size of the second abrasive is 100-500 nm, for example, it can be any point value among 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, or a range value consisting of any two point values.
[0063] In some specific embodiments of the present invention, the first abrasive includes at least one of diamond, silicon carbide, cubic boron nitride, zirconium oxide, and corundum, wherein the diamond may be single crystal, polycrystalline, or polycrystalline-like, or a combination of multiple thereof.
[0064] In some specific embodiments of the present invention, the Mohs hardness of the first abrasive is 7-10, for example, 7, 8, 9 or 10.
[0065] In some specific embodiments of the present invention, the particle size of the first abrasive is 20-500 nm, for example, it can be any point value among 20 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm or a range value consisting of any two point values.
[0066] In some specific embodiments of the present invention, the median particle size of the second abrasive is not less than the median particle size of the first abrasive, which is beneficial to improving the polishing effect.
[0067] In some specific embodiments of the present invention, the resin binder includes at least one of unsaturated polyester, epoxy resin, and polyurethane, for example, it can be epoxy acrylate, polyethylene glycol acrylate, polyurethane acrylate, bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, polyester polyurethane, polyether polyurethane, etc.
[0068] In some specific embodiments of the present invention, the filler includes one or more combinations of graphite, carbon black, carbon fiber staple fibers, carbon nanotubes, calcium carbonate, and calcium silicate, and the filler mainly serves to enhance the strength of the grinding layer.
[0069] In some specific embodiments of the present invention, the auxiliary agent includes at least one of an initiator, a curing agent, and a dispersant; for example, the initiator can be azobisisobutyronitrile, dibenzoyl peroxide, tetraphenyl glycol, tetraphenylsuccinonitrile, initiator 184, initiator 1173, initiator TPO or initiator 819, etc., which plays a role in initiating the polymerization reaction of the unsaturated polyester system; the curing agent can be aliphatic amines, aromatic amines, acid anhydrides, isocyanate curing agents, polyhydroxy curing agents, etc., which play a role in improving the crosslinking degree of the resin system and promoting the hardening and shaping of the abrasive; the dispersant can be silane coupling agents KH550, KH560, KH570, etc., which play a role in improving the interfacial bonding strength of the abrasive, filler and binder and promoting the uniform dispersion of the components.
[0070] In some specific embodiments of the present invention, the base layer is a polymer sheet, for example, the base layer polymer can be carbon fiber, PET, PC, PMMA, PS, PI, epoxy resin, phenolic resin, polyurethane, rubber elastomer or silicone elastomer.
[0071] like Figure 2 As shown, the second aspect of the present invention provides a method for preparing a grinding and polishing integrated composite abrasive tool as described in any one of the aforementioned embodiments, comprising the following steps:
[0072] S1. The raw materials of the abrasive layer are mixed and degassed to obtain a mixture, and the mixture is placed in a molding mold having a specific morphology;
[0073] S2. A base layer is applied to the non-grinding and polishing surface of the mixture, and the mixture is cured to obtain an integrated grinding and polishing composite abrasive tool; or, the mixture is first cured and demolded to obtain an abrasive layer, and then the base layer is attached to the non-grinding and polishing surface of the abrasive layer to obtain an integrated grinding and polishing composite abrasive tool.
[0074] The preparation process of the method of the present invention is simple, and the prepared integrated grinding and polishing abrasive tool can simultaneously realize integrated grinding and polishing processing, with few scratches, good surface quality, and high material removal rate. It takes into account high processing efficiency and good workpiece surface quality, and has the advantages of free abrasive processing and fixed abrasive processing.
[0075] In some specific embodiments of the present invention, the curing method is light curing or heat curing.
[0076] In some embodiments of the present invention, the UV light intensity of the photocuring is 500-1500 mW / cm 2 , for example, can be 500mW / cm2 、750mW / cm 2 , 1000mW / cm 2 、1250mW / cm 2 , 1500mW / cm 2 any point value in or a range value composed of any two point values; the irradiation time is 20-120s, for example, it can be any point value in 20s, 40s, 60s, 80s, 100s, 120s or a range value composed of any two point values.
[0077] In some specific embodiments of the present invention, the base layers are bonded by an organic adhesive or a double-sided tape. For a grinding tool containing a plurality of different base layers, the different base layers can also be bonded by an organic adhesive or a double-sided tape.
[0078] In some specific embodiments of the present invention, the organic adhesive can be one or more hot-melt or reactive adhesives, for example, epoxy resin adhesive, polyurethane resin adhesive, polyimide adhesive, organic silicone adhesive, acrylate adhesive, acrylic adhesive, etc.
[0079] In some specific embodiments of the present invention, the double-sided adhesive may be a resin-based hot melt adhesive and / or a pressure-sensitive adhesive.
[0080] The third aspect of the present invention provides a method for grinding and polishing a workpiece, wherein the workpiece is ground and polished using an integrated grinding and polishing composite abrasive tool as described in any of the aforementioned embodiments. The composite abrasive tool is used in conjunction with a water-based grinding fluid during the process of grinding and polishing the workpiece, and open holes containing a second abrasive can be formed on the surface. As the composite abrasive tool wears, the second abrasive is released layer by layer from top to bottom.
[0081] In some specific embodiments of the present invention, the material of the workpiece to be processed may be a brittle and hard material that is difficult to process, such as silicon carbide, sapphire, ceramic or special glass.
[0082] In some specific embodiments of the present invention, the water-based grinding fluid used is composed of water, an oxidant, a pH regulator, a catalyst and other components, wherein water is the main substance of the grinding fluid, which plays the role of providing a liquid environment, dissolving the pore-forming agent to form pores, and taking away the system processing heat during the processing, and the mass fraction is 80% to 98%; the oxidant is potassium permanganate, which forms a softer oxidation reaction layer on the surface of silicon carbide through an oxidation reaction to reduce the hardness of the processed workpiece, and the mass fraction is 1% to 20%; the pH regulator is one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, sodium hydroxide, potassium hydroxide, ammonia water, trimethylammonium hydroxide, etc., which plays the role of adjusting the pH of the grinding fluid and regulating the oxidizing strength of potassium permanganate, and the system pH is usually between 4 and 6 or 9 and 11. The catalyst is manganese dioxide, which can be added in the process of preparing the grinding fluid or provided by the oxidation decomposition product of potassium permanganate, and plays the role of catalytically regulating the oxidation reaction rate. Under normal circumstances, the mass fraction of manganese dioxide added is 0 to 2%.
[0083] like Figure 4 As shown, the working principle of grinding and polishing a workpiece using the above-mentioned integrated grinding and polishing composite abrasive tool is as follows: During the grinding and polishing process, the oxidant in the water-based grinding fluid reacts chemically with the workpiece surface under the action of a catalyst to generate a softened film layer with a hardness lower than that of the workpiece; at the same time, the water-soluble adhesive in the organic microsphere pore-forming agent on the surface of the abrasive tool contacts and dissolves with water, forming spherical or nearly spherical open holes on the surface of the composite abrasive tool, and the holes contain free second abrasives; the first abrasive and the second abrasive in the abrasive layer play a role in mechanically removing the softened film layer on the workpiece surface. Among them, the first abrasive has a higher hardness than the second abrasive and mainly plays a role in material removal, while the second abrasive mainly plays a role in polishing.
[0084] The following is a detailed description of some embodiments of the present invention in conjunction with specific examples. The raw materials used in the examples can be purchased from the market unless otherwise specified.
[0085] In Examples 1-8, the first abrasive d 50 The particle size is 200nm; the particle size of the organic composite microsphere pore-forming agent is 32-38μm, all of which are obtained by centrifugal spray granulation. 50 The particle size is 250nm. The median particle size of the filler used is 0.5μm; the unsaturated polyester used is a mixture of prepolymer PEG400DA and a crosslinker, the epoxy resin is urethane-modified epoxy resin UME308, and the polyurethane is a mixture of polyester-type polyurethane prepolymer and diethylenetriamine; wherein the dispersant used in the unsaturated polyester system is KH570, the dispersant used in the epoxy resin system is KH560, and the dispersant used in the polyurethane system is KH550. The formulation composition of the abrasive layer in Examples 1-8 is shown in Table 1.
[0086] Table 1
[0087]
[0088] Example 1
[0089] The formula composition of the abrasive layer of this embodiment is shown in Table 1. The base layer adopts a PET sheet with a thickness of 0.15 mm. The preparation method of the grinding and polishing integrated composite abrasive tool is as follows:
[0090] S1. The abrasive layer raw materials weighed in accordance with the ratio in Table 1 are mixed evenly, degassed and cast in a molding mold having a specific morphology;
[0091] S2. Place the molding mold in a blast oven and use thermal curing to form and cure it. The curing procedure is 80℃ / 2h+100℃ / 2h+120℃ / 1h. After curing and demoulding, an abrasive layer is obtained. The PET base layer is attached to the non-grinding surface of the abrasive layer with double-sided tape to obtain an integrated grinding and polishing composite abrasive tool.
[0092] Example 2
[0093] The formulation of the abrasive layer in this embodiment is shown in Table 1. The base layer adopts a PET sheet with a thickness of 0.15 mm. The preparation method of the integrated grinding and polishing composite abrasive tool is the same as that in Example 1.
[0094] Example 3
[0095] The formula composition of the abrasive layer of this embodiment is shown in Table 1. The base layer adopts a 0.2 mm thick polyurethane sheet. The preparation method of the grinding and polishing integrated composite abrasive tool is as follows:
[0096] S1. The abrasive layer raw materials weighed in accordance with the ratio in Table 1 are mixed evenly, degassed and cast in a molding mold having a specific morphology;
[0097] S2. Place the molding mold in a blast oven and use thermal curing to cure the mold. The curing procedure is 80℃ / 2h+100℃ / 2h+140℃ / 2h. After curing and demoulding, an abrasive layer is obtained. The polyurethane base layer is attached to the non-grinding surface of the abrasive layer with double-sided tape to obtain an integrated grinding and polishing composite abrasive tool.
[0098] Example 4
[0099] The formula composition of the abrasive layer in this embodiment is shown in Table 1. The base layer adopts a 0.2 mm thick polyurethane sheet. The preparation method of the integrated grinding and polishing composite abrasive tool is the same as that in Example 3.
[0100] Example 5
[0101] The formula composition of the abrasive layer of this embodiment is shown in Table 1. The base layer adopts a 0.15 mm thick PC sheet. The preparation method of the grinding and polishing integrated composite abrasive tool is as follows:
[0102] S1. The abrasive layer raw materials weighed in accordance with the ratio in Table 1 are mixed evenly, degassed and cast in a molding mold having a specific morphology;
[0103] S2. Paste the PC substrate layer sheet on the non-grinding and polishing surface of the molding material, degas again, place the molding mold in a blast oven, and sinter and cure and demold through a program to obtain an integrated grinding and polishing composite abrasive tool; wherein the curing program is 60℃ / 30min.
[0104] Example 6
[0105] The formulation of the abrasive layer in this embodiment is shown in Table 1. The base layer adopts a 0.15 mm thick PC sheet. The preparation method of the integrated grinding and polishing composite abrasive tool is the same as that in Example 5.
[0106] Example 7
[0107] The formula composition of the abrasive layer of this embodiment is shown in Table 1. The base layer adopts a PET sheet with a thickness of 0.15 mm. The preparation method of the grinding and polishing integrated composite abrasive tool is as follows:
[0108] S1. The abrasive layer raw materials weighed in accordance with the ratio in Table 1 are mixed evenly, degassed and cast in a molding mold having a specific morphology;
[0109] S2. The PET substrate sheet is pasted on the non-polished surface of the molding material, degassed again, cured and demolded by a light curing process to obtain a grinding and polishing integrated composite abrasive tool; wherein the light curing process uses a light intensity of 1000mW / cm 2 The samples were irradiated with UV light for 80 s.
[0110] Example 8
[0111] The formula composition of the abrasive layer in this embodiment is shown in Table 1, and the base layer adopts a 0.15 mm thick PET sheet; the preparation method of the integrated grinding and polishing composite abrasive tool is the same as that of Example 7.
[0112] Comparative Example 1
[0113] Comparative Example 1 is similar to Example 1, except that no organic composite microsphere pore-forming agent is added to the abrasive layer of Comparative Example 1, and the ratios of other components remain unchanged. The base layer and abrasive tool preparation method used are the same as in Example 1.
[0114] Comparative Example 2
[0115] Comparative Example 2 is similar to Example 3, except that no organic composite microsphere pore-forming agent is added to the abrasive layer of Comparative Example 2, and the ratios of other components remain unchanged. The base layer and abrasive tool preparation method used are the same as those in Example 3.
[0116] Comparative Example 3
[0117] Comparative Example 3 is similar to Example 5, except that no organic composite microsphere pore-forming agent is added to the abrasive layer of Comparative Example 3, and the ratios of other components remain unchanged. The base layer and abrasive tool preparation methods used are the same as those of Example 5.
[0118] Comparative Example 4
[0119] Comparative Example 4 is similar to Example 1, except that alumina is replaced with an equal amount of dextrin (dextrin content is 25wt%, alumina content is 0), dextrin microspheres without a second abrasive are used instead of the organic composite microsphere pore-forming agent in Example 1, and the other conditions are the same as those in Example 1.
[0120] Comparative Example 5
[0121] Comparative Example 5 is similar to Example 1, except that dextrin is replaced with an equal amount of alumina (dextrin content is 0, alumina content is 25 wt%), and the second abrasive is used instead of the organic composite microsphere pore-forming agent in Example 1. The other conditions are the same as those in Example 1.
[0122] Comparative Example 6
[0123] Comparative Example 6 is similar to Example 1, except that dextrin (water-soluble binder) and alumina (second abrasive) are not granulated, the content of each component is the same as that in Example 1, all raw materials are directly mixed to prepare a composite abrasive tool, and the other process conditions are the same as those in Example 1.
[0124] Test example
[0125] (1) Density, dry hardness and abrasive surface pore size test
[0126] The density and dry hardness of the abrasive layer of the composite abrasive tool prepared in each embodiment and each comparative example were tested respectively, and the pore size of the holes formed on the surface of the composite abrasive tool after the water-soluble binder in the organic composite microsphere pore-forming agent was dissolved was tested;
[0127] Density, measured by density tester, the test liquid medium is kerosene;
[0128] Dry hardness: the water-soluble binder in the organic microsphere pore-forming agent on the surface of the abrasive layer is not dissolved, and the hardness data is measured by a Shore C hardness tester;
[0129] The pore size is determined by dissolving the water-soluble binder in the organic composite microsphere pore-forming agent on the surface of the abrasive layer in water and then drying it, and then placing it at room temperature for 24 hours. The pore size data are measured by SEM, and the average value of 20 pore size data in the same area is taken.
[0130] The test results are shown in Table 2.
[0131] Table 2
[0132] <![CDATA[Density (g / cm 3 )]]> Dry hardness Pore size (μm) Example 1 1.59±0.10 82±4 34±5 Example 2 1.70±0.10 79±4 33±4 Example 3 1.43±0.11 74±3 34±4 Example 4 1.39±0.10 78±4 33±5 Example 5 1.62±0.12 72±5 33±4 Example 6 1.66±0.11 69±4 34±5 Example 7 1.60±0.13 72±5 34±3 Example 8 1.59±0.10 68±3 33±4 Comparative Example 1 1.40±0.09 83±3 / Comparative Example 2 1.30±0.10 76±4 / Comparative Example 3 1.31±0.08 74±3 / Comparative Example 4 1.17±0.09 79±5 33±6 Comparative Example 5 1.64±0.12 85±6 / Comparative Example 6 1.62±0.16 81±4 /
[0133] It can be seen from the data in Table 2 that when the dry abrasive layer is not porous inside, the density of the abrasive layer is related to the composition ratio in the formula. When the proportions of other components do not change much, the density change of the abrasive layer of the abrasive tool with the addition of organic microsphere pore-forming agent is mainly affected by the type and content of each component in the organic microsphere pore-forming agent. It can be seen from Example 1 and Comparative Example 6 that when the formula composition is the same, the density of the abrasive layer of the composite abrasive tool prepared by adding the organic composite microsphere pore-forming agent is not much different from that of the abrasive tool prepared by mixing all the raw materials (not granulated).
[0134] By comparing Example 1 with Comparative Example 1, Example 3 with Comparative Example 2, and Example 5 with Comparative Example 3, it can be seen that the introduction of the organic composite microsphere pore-forming agent in the examples will slightly reduce the hardness of the abrasive layer. By comparing Example 1 with Examples 7 to 8, it can be seen that by reducing the proportion of the first abrasive and increasing the proportion of the organic composite microsphere pore-forming agent, the hardness of the abrasive layer is significantly reduced.
[0135] It can be seen from Examples 1 to 8 that the pore size on the surface of the abrasive layer is similar to the diameter of the organic composite microsphere pore-forming agent, and the pore size on the surface of the abrasive layer formed by the method is relatively uniform.
[0136] (2) Polishing performance test
[0137] During the grinding and polishing process, the grinding tools of Examples 1, 3, 5, 7, 8 and Comparative Examples 1 to 6 were used in combination with abrasive-free grinding and polishing liquid (KMnO4 polishing liquid, pH = 5.2 to 5.8);
[0138] Comparative Example 7 is an example of using SUBA800 as a polishing pad and a 250nm silica polishing liquid (pH = 10.0-10.5, abrasive solid content 2wt%) to perform free abrasive processing;
[0139] Comparative Example 8 is an example of using SUBA800 as a polishing pad and a diamond polishing liquid (KMnO4 polishing liquid, pH = 5.2-5.8, abrasive solid content 2wt%) with a particle size of 200nm to perform free abrasive processing;
[0140] The test process is as follows Figure 6 As shown, the grinding tools in Examples 1, 3, 5, 7, 8 and Comparative Examples 1 to 8 are fixed on a turntable, a 4-inch SiC single crystal wafer is fixed on a workpiece carrier (Si side facing downward), and the grinding and polishing liquid is supplied through a liquid supply device. Other processing parameters are shown in Table 3.
[0141] Table 3
[0142]
[0143]
[0144] The average material removal rate, surface roughness, intra-chip non-uniformity, and average abrasive consumption rate of the grinding and polishing process of each embodiment and each comparative example were tested as indicators for evaluating the grinding and polishing effect;
[0145] The average material removal efficiency was calculated using the mass method;
[0146] Surface roughness was measured using white light interferometry;
[0147] On-wafer non-uniformity measurement: 17 points are evenly selected along two mutually perpendicular diameters on the wafer processing surface, from the wafer edge, through the center to the other edge, and the thickness H is measured. Calculation formula: Non-uniformity = (H max -H min ) / (2×H 均值 )×100%;
[0148] Calculation method of average abrasive consumption rate: In Examples 1, 3, 5, 7, 8 and Comparative Examples 1 to 6, average abrasive consumption rate = abrasive consumption of prepared abrasive tool / abrasive tool life; in Comparative Examples 7 to 8, average abrasive consumption rate = polishing liquid flow rate × polishing liquid density × abrasive mass fraction in the polishing liquid.
[0149] The test results are shown in Table 4.
[0150] Table 4
[0151]
[0152] From the data in Table 4, it can be seen that the composite abrasive tool (Examples 1, 3, 5) prepared by the embodiment of the present invention has a higher average material removal rate and a lower workpiece surface roughness than the abrasive tool with the same formula (Comparative Examples 1-3) without organic composite microsphere pore-forming agent, which can take into account both processing efficiency and surface quality; By comparing Example 1 with Comparative Examples 4-6, it can be seen that the realization of the processing effect of the present invention depends on the introduction of the organic composite microsphere pore-forming agent, and the same processing effect cannot be achieved by simply mixing part or all of the raw materials of the organic composite microsphere pore-forming agent in the abrasive layer; that is, even if the formula composition is consistent, if the second abrasive and the water-soluble adhesive are directly mixed with other raw materials to prepare the abrasive tool, and the second abrasive and the water-soluble adhesive are not granulated in advance to prepare them into organic composite microsphere pore-forming agents, the effect of the present invention cannot be achieved. Compared with the free processing scheme of the same kind of processing abrasive (Comparative Examples 7-8), the method of the present invention has a higher material removal efficiency, the processed workpiece has better intra-sheet uniformity, and has a lower abrasive consumption rate per unit time, which is conducive to reducing the pollution of processing waste liquid to the environment.
[0153] From the comparison between Example 7 and Example 8, it can be seen that reducing the proportion of the first abrasive and increasing the proportion of the organic composite microsphere pore-forming agent reduces the average material removal efficiency of the workpiece but is beneficial to improving the roughness of the workpiece surface.
[0154] From the above discussion, it can be seen that the integrated grinding and polishing composite abrasive tool prepared by the method of the present invention can achieve a better comprehensive effect of material removal rate and surface quality, and at the same time can significantly improve the processing uniformity of silicon carbide workpieces and reduce the pollution of processing waste liquid to the environment.
[0155] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A grinding and polishing integrated composite abrasive tool, characterized in that: It comprises a base layer and an abrasive layer, wherein the abrasive layer is solidified with a first abrasive and an organic composite microsphere pore-forming agent, the organic composite microsphere pore-forming agent is a spherical or nearly spherical composite comprising a second abrasive and a water-soluble adhesive, and the hardness of the second abrasive is less than or equal to the hardness of the first abrasive.
2. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: In terms of mass percentage, the abrasive layer comprises 30%-60% of a resin binder, 3%-20% of the first abrasive, 3%-35% of the organic composite microsphere pore-forming agent, 3%-10% of a filler and 0.2%-15% of an auxiliary agent.
3. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: Contains at least one of the following characteristics: (1) The particle size of the organic composite microsphere pore-forming agent is 20-90 μm; (2) In the organic composite microsphere pore-forming agent, the mass percentage of the water-soluble adhesive is 2.5%-10%; (3) The preparation method of the organic composite microsphere pore-forming agent includes one of centrifugal spray granulation, rolling granulation or reverse microemulsion polymerization.
4. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: The water-soluble adhesive includes at least one of cyclodextrin, dextrin, starch, hydroxymethyl cellulose, methyl cellulose, polyacrylic acid, polyacrylamide, and polyvinyl alcohol.
5. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: Contains at least one of the following characteristics: (1) The second abrasive comprises at least one of aluminum oxide, silicon dioxide, and cerium oxide; (2) the Mohs hardness of the second abrasive is 6-9; (3) The particle size of the second abrasive is 100-500 nm.
6. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: Contains at least one of the following characteristics: (1) The first abrasive includes at least one of diamond, silicon carbide, cubic boron nitride, zirconium oxide, and corundum; (2) The Mohs hardness of the first abrasive is 7-10; (3) The particle size of the first abrasive is 20-500 nm.
7. The grinding and polishing integrated composite abrasive tool according to claim 1, characterized in that: The median particle size of the second abrasive is not less than the median particle size of the first abrasive.
8. The grinding and polishing integrated composite abrasive tool according to claim 2, characterized in that: Contains at least one of the following characteristics: (1) The resin binder includes at least one of unsaturated polyester, epoxy resin, and polyurethane; (2) The filler includes at least one of graphite, carbon black, carbon fiber staple fibers, carbon nanotubes, calcium carbonate, and calcium silicate; (3) The auxiliary agent includes at least one of an initiator, a curing agent, and a dispersant.
9. The method for preparing the grinding and polishing integrated composite abrasive tool according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. The raw materials of the abrasive layer are mixed and degassed to obtain a mixture, and the mixture is placed in a molding mold; S2. A base layer is applied to the non-grinding and polishing surface of the mixture, and the grinding and polishing integrated composite abrasive tool is obtained through solidification; or, the mixture is first solidified to obtain an abrasive layer, and then the base layer is adhered to the non-grinding and polishing surface of the abrasive layer to obtain the grinding and polishing integrated composite abrasive tool.
10. A method for grinding and polishing a workpiece, characterized in that: The workpiece is ground and polished using the integrated grinding and polishing composite abrasive tool as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Self-lubricating grinding tool and preparation method thereof
CN101758463A
Method for manufacturing soluble fixed soft abrasive-polishing film
CN104209879A
High-self-sharpening grinding pad
CN109571296A
Abrasive article, a process for its manufacture, and a method of using it to reduce a workpiece surface
CN1102800A
Grinding pad for photocatalysis-assisted chemical mechanical polishing and preparation method thereof
CN115674008A
Cited By
Preparation method of slotting-free polishing disc
CN119635526A