Carbon fiber spoke disc forming process
By using a carbon fiber spoke disc molding process, which involves high-temperature molding with carbon fiber material and specific molds, the problem of excessive weight of metal spoke discs has been solved, thus achieving lightweighting of carbon fiber bicycles.
Patent Information
- Application Number
- CN202411203050.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing carbon fiber bicycles typically use metal spokes and chainrings, which increases the weight of the bicycle.
The carbon fiber spoke disc is formed using a carbon fiber material molding process. The spoke disc is made of carbon fiber material and formed through a specific mold and high-temperature baking process. Combined with flexible pressure blocks and air bags for uniform pressure distribution, a lightweight carbon fiber spoke disc is formed.
The produced carbon fiber spoke discs are lighter than traditional metal spoke discs, with uniform wall thickness, achieving a lightweight effect.
Smart Images

Figure CN118927667A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber bicycles, in particular to a carbon fiber spoke disc molding process. Background Art
[0002] Carbon fiber bicycles, as the name suggests, refer to bicycles whose key components such as the frame, front fork, and wheels are mainly made of carbon fiber materials. Carbon fiber is a new type of composite material with the advantages of light weight, high specific strength, high specific stiffness, and good corrosion resistance, which makes carbon fiber bicycles perform well in performance.
[0003] At present, the spoke discs of carbon fiber bicycles are usually made of metal materials, but the weight of metal materials is relatively large, which increases the weight of carbon fiber bicycles. Therefore, a carbon fiber spoke disc is urgently needed to replace the metal spoke disc to reduce the weight of carbon fiber bicycles. Summary of the invention
[0004] The object of the present invention is to provide a carbon fiber spoke disc molding process to solve the problem of excessive weight of metal spoke discs.
[0005] To achieve the above object, the present invention discloses a carbon fiber spoke disc forming process, comprising the following steps:
[0006] S1. Preform a carbon fiber spoke wheel blank.
[0007] S2, placing the spoke disc rough blank into a carbon fiber spoke disc forming mold for secondary molding.
[0008] The carbon fiber spoke disc forming mold comprises:
[0009] A first upper mold, a first lower mold, a first wedge block, a mold core, a flexible pressure block and an air bag; the first upper mold is arranged directly above the first lower mold, the flexible pressure block is arranged between the first upper mold and the first lower mold, the first wedge block is arranged between the flexible pressure block and the first lower mold, a plug-in groove is provided in the middle of the upper surface of the first lower mold, the mold core cooperates with the plug-in groove, a first molding surface is provided on the top of the first lower mold, and a second molding surface is provided on the bottom of the flexible pressure block; an installation groove is provided at the bottom of the first upper mold, the air bag is installed in the installation groove, and the air bag is connected to an external air source.
[0010] Placing the spoke disc rough blank into the carbon fiber spoke disc forming mold comprises the following steps:
[0011] a1. Insert the first wedge block on the circumference of the carbon fiber spoke disc blank.
[0012] a2. Place the first wedge together with the carbon fiber spoke disc rough blank into the first lower mold.
[0013] a3. Pass the mold core through the carbon fiber spoke disc rough blank and insert it into the insertion groove.
[0014] a4. Place the flexible pressing block on the carbon fiber spoke disc rough blank.
[0015] a5. Combine the first upper mold containing the air bag with the first lower mold.
[0016] a6. Place the installed carbon fiber spoke disk forming mold on a forming furnace for high temperature baking, and at the same time, inflate the air bag and maintain the air pressure in the air bag.
[0017] a7. After the baking is finished, the carbon fiber spoke disc forming mold is opened to obtain the carbon fiber spoke disc.
[0018] Preferably, in step a6, the carbon fiber spoke disk forming mold is placed on a forming furnace and baked at 150° C. for 1 hour, and the forming pressure of the forming furnace is 1±0.2 MPa.
[0019] Preferably, in step a6, the pressure of the air bag is maintained at 8-10 kg.
[0020] Preferably, a boss is fixedly connected to the top of the first lower mold, the first molding surface is arranged on the boss, and a plurality of the first wedge blocks are arranged around the boss; the first wedge block includes a base and a plug-in portion, the plug-in portion is fixedly connected to one side of the top of the base, and after the base is fitted with the side surface of the boss, the plug-in portion is located above the first molding surface.
[0021] Preferably, a slide groove is provided at the bottom of the first wedge block, and a slide rail is provided at the top of the first lower mold. The straight line where the slide rail is located passes through the center of the boss, and the slide rail is slidably connected to the slide groove.
[0022] Preferably, the cross-sectional shape of the mold core is a regular polygon.
[0023] Preferably, the flexible pressing block is made of rubber or silicone.
[0024] Preferably, the air bag is provided with an air nozzle, the air nozzle is connected to the outside, a through hole for installing the air nozzle is opened on one side of the upper mold, and the air nozzle passes through the through hole.
[0025] Preferably, the carbon fiber spoke disk rough blank is formed on a carbon fiber spoke disk preforming jig, and the carbon fiber spoke disk forming jig comprises a second lower mold, a second wedge block and a second upper mold, wherein the second upper mold is arranged directly above the second lower mold, and the second wedge block is arranged between the second lower mold and the second upper mold; a third molding surface is provided on the upper surface of the second lower mold, and a hole molding column is provided in the middle of the upper surface of the second lower mold; a fourth molding surface is provided on the lower surface of the second wedge block, and a fifth molding surface is provided on the upper surface of the second wedge block; a first plug hole is provided in the middle of the lower surface of the second upper mold, and the hole molding column cooperates with the first plug hole.
[0026] Preferably, the carbon fiber spoke disk rough blank comprises: a disk body made of carbon fiber material, a mounting hole is opened in the middle of the disk body, the periphery of the disk body is composed of a first carbon fiber sheet and a second carbon fiber sheet, an installation space for embedding spokes is formed between the first carbon fiber sheet and the second carbon fiber sheet, the installation space comprises a first embedding groove and a second embedding groove, the first embedding groove and the second embedding groove are alternately arranged along the circumference of the disk body, and the width e of the second embedding groove is greater than the width f of the first embedding groove.
[0027] Preferably, in step S1, preforming the carbon fiber spoke disc blank comprises the following steps:
[0028] b1. Laying carbon yarn on the third molding surface of the second lower mold to form the first fiber sheet of the carbon fiber spoke disk.
[0029] b2. Install the second wedge block on the first fiber sheet of the carbon fiber spoke disc so that the upper surface of the first fiber sheet of the carbon fiber spoke disc is in contact with the fourth molding surface.
[0030] b3. Carbon yarn is laid on the fifth forming surface to form a second fiber sheet of the carbon fiber spoke disk. One side of the second fiber sheet is fixedly connected to the first fiber sheet, and the other side is separated from the first fiber sheet, so that an installation space is formed between the first fiber sheet and the second fiber sheet.
[0031] b4. Install the second upper mold on the top of the second fiber sheet to fix the carbon yarn wound in the jig.
[0032] b5. After fixing for a period of time, disassemble the mold to obtain the rough blank of the carbon fiber spoke disc.
[0033] Preferably, in step b5, the fixing time of the carbon yarn in the carbon fiber spoke disc preforming jig is half an hour.
[0034] The present invention has the following beneficial effects:
[0035] The carbon fiber spoke disc produced by the process of the present invention is lighter in weight than a traditional metal spoke disc. At the same time, during the molding process of the carbon fiber spoke disc, a flexible rubber mold is used to cover the carbon fiber spoke disc. The rubber mold can be completely fitted with the carbon fiber spoke disc under the action of pressure, so that the pressure from the air bag is evenly dispersed on the carbon fiber spoke disc, thereby making the wall thickness of the carbon fiber spoke disc thinner and more uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is an exploded schematic diagram of a carbon fiber spoke disc forming mold provided in a specific embodiment of the present invention;
[0037] Figure 2 This is a schematic diagram of the overall structure of a carbon fiber spoke disc forming mold provided in a specific embodiment of the present invention;
[0038] Figure 3 It is a cross-sectional schematic diagram of a carbon fiber spoke disc forming mold provided in a specific embodiment of the present invention;
[0039] Figure 4 It is an exploded schematic diagram of a carbon fiber spoke disc preforming jig provided in a specific embodiment of the present invention;
[0040] Figure 5 It is a schematic diagram of the overall structure of a carbon fiber spoke disc preforming jig provided in a specific embodiment of the present invention;
[0041] Figure 6 It is a schematic diagram of the overall structure of a carbon fiber spoke disc provided in a specific embodiment of the present invention;
[0042] Figure 7 It is a schematic side view of a carbon fiber spoke disc provided in a specific embodiment of the present invention.
[0043] Main component symbols:
[0044] 100, first lower mold; 110, boss; 111, first molding surface; 112, plug-in slot; 120, slide rail; 200, first wedge block; 210, base; 220, plug-in portion; 230, slide slot; 300, molding column; 400, flexible pressure block; 500, air bag; 510, air nozzle; 600, first upper mold; 610, through hole; 620, mounting slot; 700, carbon fiber spoke disk; 701, first embedding slot; 702, second embedding slot; 710, first carbon fiber sheet; 720, second carbon fiber sheet; 730, mounting hole; 800, second lower mold; 801, third molding surface; 802, hole molding column; 810, second wedge block; 811, fifth molding surface; 820, second upper mold. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0046] like Figures 1 to 7 As shown, the present invention discloses a carbon fiber spoke disc forming process, comprising the following steps:
[0047] S1. Preform a carbon fiber spoke disc 700 rough blank.
[0048] The rough blank of the carbon fiber spoke disk 700 includes: a disk body made of carbon fiber material, a mounting hole 730 is opened in the middle of the disk body, the periphery of the disk body is composed of a first carbon fiber sheet 710 and a second carbon fiber sheet 720, an installation space for embedding the spokes is formed between the first carbon fiber sheet 710 and the second carbon fiber sheet 720, the installation space includes a first embedding groove 701 and a second embedding groove 702, the first embedding groove 701 and the second embedding groove 702 are alternately arranged along the circumference of the disk body, and the width e of the second embedding groove 702 is greater than the width f of the first embedding groove 701.
[0049] S2. Place the spoke disc blank into the carbon fiber spoke disc 700 molding die for secondary molding.
[0050] Carbon fiber spoke disc 700 molding mold includes:
[0051] The first upper mold 600, the first lower mold 100, the first wedge block 200, the mold core, the flexible pressure block 400 and the air bag 500; the first upper mold 600 is arranged directly above the first lower mold 100, the flexible pressure block 400 is arranged between the first upper mold 600 and the first lower mold 100, the first wedge block 200 is arranged between the flexible pressure block 400 and the first lower mold 100, a plug-in groove 112 is provided in the middle of the upper surface of the first lower mold 100, the mold core cooperates with the plug-in groove 112, the top of the first lower mold 100 is provided with a first molding surface 111, and the bottom of the flexible pressure block 400 is provided with a second molding surface; the bottom of the first upper mold 600 is provided with a mounting groove 620, the air bag 500 is installed in the mounting groove 620, and the air bag 500 is connected to an external air source.
[0052] Placing the spoke disc rough blank into the carbon fiber spoke disc 700 forming mold comprises the following steps:
[0053] a1, insert the first wedge block 200 on the circumference of the rough carbon fiber spoke disc 700. That is, insert the first wedge block 200 into the first embedding groove 701 and the second embedding groove 702.
[0054] a2. Put the first wedge 200 together with the rough carbon fiber spoke disc 700 into the first lower mold 100 so that the first molding surface 111 is consistent with the lower surface of the carbon fiber spoke disc 700.
[0055] a3. Pass the mold core through the mounting hole 730 of the rough carbon fiber spoke disc 700 and insert it into the insertion groove 112.
[0056] a4. Place the flexible pressing block 400 on the rough carbon fiber spoke disc 700.
[0057] a5. Combine the first upper mold 600 equipped with the air bag 500 with the first lower mold 100.
[0058] a6. Place the assembled carbon fiber spoke disc 700 forming mold on a forming furnace for high temperature baking, and at the same time, inflate the air bag 500 and maintain the air pressure in the air bag 500.
[0059] a7. After the baking is finished, the carbon fiber spoke disc 700 forming mold is opened to obtain the carbon fiber spoke disc 700.
[0060] In this embodiment, in step a6, the carbon fiber spoke disc 700 forming mold is placed on a forming furnace and baked at 150° C. for 1 hour, and the forming furnace forming pressure is 1±0.2 MPa. The pressure of the air bag 500 is maintained at 8-10 kg.
[0061] In this embodiment, the flexible pressing block 400 is made of rubber or silicone, and the second molding surface at the bottom of the flexible pressing block 400 fits the top of the carbon fiber spoke disc 700. The flexible pressing block 400 is used to cover the rough carbon fiber spoke disc 700. Under the action of pressure, the flexible pressing block 400 can be completely fitted with the carbon fiber spoke disc 700, so that the pressure from the air bag 500 is evenly dispersed on the carbon fiber spoke disc 700, so that the wall thickness of the carbon fiber spoke disc 700 becomes thinner and more uniform, thereby achieving the purpose of lightweighting the carbon fiber spoke disc 700.
[0062] A boss 110 is fixedly connected to the top of the first lower mold 100, a first molding surface 111 is arranged on the boss 110, and a plurality of first wedge blocks 200 are arranged around the boss 110; the first wedge block 200 includes a base 210 and a plug-in portion 220, the plug-in portion 220 is fixedly connected to one side of the top of the base 210, and after the base 210 is fitted with the side of the boss 110, the plug-in portion 220 is located above the first molding surface 111.
[0063] In this embodiment, a slide groove 230 is provided at the bottom of the first wedge block 200, and a slide rail 120 is provided at the top of the first lower mold 100. The straight line where the slide rail 120 is located passes through the center of the boss 110, and the slide rail 120 is slidably connected with the slide groove 230. During use, the first wedge block 200 is arranged in the installation space on the side of the preformed carbon fiber spoke disk 700 in a specific order to assist in the molding of the first embedding groove 701 and the second embedding groove 702 on the side of the carbon fiber spoke disk 700. The slide rail 120 and the slide groove 230 cooperate with each other to assist in positioning the first wedge block 200, prevent the first wedge block 200 from shaking and rotating, and also facilitate and accurately guide the first wedge block 200 to enter or exit the installation space on the side of the carbon fiber spoke disk 700.
[0064] The cross-sectional shape of the mold core is a regular polygon. In this embodiment, the cross-sectional shape of the mold core is a regular hexagon, and the corners of the mold core are provided with rounded corners. The mold core is used to form the mounting hole 730 in the middle of the carbon fiber spoke disk 700, and the mounting hole 730 is connected to the shaft on the hub. The mounting hole 730 is formed into a hexagon by the mold core, which can prevent the carbon fiber spoke disk 700 from rotating relative to the shaft.
[0065] The air bag 500 is provided with an air nozzle 510, which is connected to the outside. A through hole 610 for installing the air nozzle 510 is provided on one side of the upper mold, and the air nozzle 510 passes through the through hole 610. In this embodiment, during use, the first upper mold 600 and the first lower mold 100 are locked by bolts. The high-pressure gas source enters the air bag 500 through the air nozzle 510 to inflate and maintain the pressure of the air bag 500. After the air bag 500 is inflated, a pressure of 8-10 kg is provided for the flexible pressing block 400.
[0066] The rough carbon fiber spoke disc 700 is formed on a carbon fiber spoke disc preforming jig, and the carbon fiber spoke disc 700 forming jig includes a second lower die 800, a second wedge block 810 and a second upper die 820, wherein the second upper die 820 is arranged directly above the second lower die 800, and the second wedge block 810 is arranged between the second lower die 800 and the second upper die 820; a third forming surface 801 is provided on the upper surface of the second lower die 800, and a hole forming column 802 is provided in the middle of the upper surface of the second lower die 800; a fourth forming surface is provided on the lower surface of the second wedge block 810, and a fifth forming surface 811 is provided on the upper surface of the second wedge block 810. A first plug hole is provided in the middle of the lower surface of the second upper die 820, and the hole forming column 802 matches the first plug hole.
[0067] In this embodiment, the carbon fiber spoke disc 700 is disc-shaped when viewed from above, with a polygonal mounting hole 730 in the middle and a mounting space for mounting spokes on its side. The carbon yarn is wound and fixed on the outside of the hole forming column 802 to form the mounting hole 730. The second wedge block 810 is used to assist the rough carbon fiber spoke disc 700 in forming the mounting space. The second wedge block 810 is semicircular, and there are two second wedge blocks 810. The two second wedge blocks 810 form a circular ring and are inserted on the side of the rough carbon fiber spoke disc 700.
[0068] In step S1, preforming of the rough carbon fiber spoke disc 700 includes the following steps:
[0069] b1. Laying carbon yarn on the third molding surface 801 of the second lower mold 800 to form a first fiber sheet of the carbon fiber spoke disk 700.
[0070] b2. Install the second wedge block 810 on the first fiber sheet of the carbon fiber spoke disc 700 so that the upper surface of the first fiber sheet of the carbon fiber spoke disc 700 is in contact with the fourth molding surface.
[0071] b3. Carbon yarn is laid on the fifth molding surface 811 to form a second fiber sheet of the carbon fiber spoke disk 700. One side of the second fiber sheet is fixedly connected to the first fiber sheet, and the other side is separated from the first fiber sheet, so that an installation space is formed between the first fiber sheet and the second fiber sheet.
[0072] b4. Install the second upper mold 820 on the top of the second fiber sheet to fix the carbon yarn wound in the jig.
[0073] b5. After fixing for a period of time, disassemble the mold to obtain the carbon fiber spoke disc 700 rough blank.
[0074] In this embodiment, in step b5, the fixing time of the carbon yarn in the carbon fiber spoke disk preforming jig is half an hour.
[0075] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A carbon fiber spoke disc forming process, characterized in that: The following steps are involved: S1, preforming a rough blank of a carbon fiber spoke disc (700); S2, placing the spoke disc rough blank into a carbon fiber spoke disc (700) forming mold for secondary forming; The carbon fiber spoke disc (700) forming die comprises: A first upper mold (600), a first lower mold (100), a first wedge block (200), a mold core, a flexible pressure block (400) and an air bag (500); the first upper mold (600) is arranged directly above the first lower mold (100), the flexible pressure block (400) is arranged between the first upper mold (600) and the first lower mold (100), the first wedge block (200) is arranged between the flexible pressure block (400) and the first lower mold (100), and the first A plug-in groove (112) is provided in the middle of the upper surface of the lower mold (100), the mold core cooperates with the plug-in groove (112), a first molding surface (111) is provided at the top of the first lower mold (100), and a second molding surface is provided at the bottom of the flexible pressure block (400); a mounting groove (620) is provided at the bottom of the first upper mold (600), the air bag (500) is installed in the mounting groove (620), and the air bag (500) is connected to an external air source; Placing the spoke disc rough blank into a carbon fiber spoke disc (700) forming mold comprises the following steps: a1. inserting the first wedge (200) on the peripheral side of the rough carbon fiber spoke disk (700); a2. Place the first wedge (200) together with the rough carbon fiber spoke disc (700) into the first lower mold (100); a3, passing the mold core through the rough blank of the carbon fiber spoke disc (700), and inserting it into the insertion groove (112); a4, placing the flexible pressing block (400) on the rough blank of the carbon fiber spoke disc (700); a5. Combining the first upper mold (600) equipped with the air bag (500) with the first lower mold (100); a6. placing the installed carbon fiber spoke disc (700) forming mold on a forming furnace for high temperature baking, and at the same time inflating the air bag (500) and maintaining the air pressure in the air bag (500); a7. After the baking is finished, the carbon fiber spoke disc (700) forming mold is opened to obtain the carbon fiber spoke disc (700).
2. A carbon fiber spoke disc forming process according to claim 1, characterized in that: In step a6, the carbon fiber spoke disc (700) forming mold is placed on a forming furnace and baked at 150° C. for 1 hour, and the forming pressure of the forming furnace is 1±0.2 MPa.
3. A carbon fiber spoke disc forming process according to claim 2, characterized in that: In step a6, the pressure of the air bag (500) is maintained at 8-10 kg.
4. A carbon fiber spoke disc forming process according to claim 3, characterized in that: The top of the first lower mold (100) is fixedly connected to a boss (110), the first molding surface (111) is arranged on the boss (110), and a plurality of the first wedge blocks (200) are arranged around the boss (110); the first wedge block (200) comprises a base (210) and an inserting portion (220), the inserting portion (220) is fixedly connected to one side of the top of the base (210), and after the base (210) is fitted with the side surface of the boss (110), the inserting portion (220) is located above the first molding surface (111).
5. A carbon fiber spoke disc forming process according to claim 4, characterized in that: A slide groove (230) is provided at the bottom of the first wedge block (200), and a slide rail (120) is provided at the top of the first lower mold (100). The straight line where the slide rail (120) is located passes through the center of the boss (110), and the slide rail (120) is slidably connected to the slide groove (230).
6. A carbon fiber spoke disc forming process according to claim 5, characterized in that: The cross-sectional shape of the mold core is a regular polygon.
7. The carbon fiber spoke disc forming process according to claim 1, characterized in that: The flexible pressing block (400) is made of rubber or silicone.
8. The carbon fiber spoke disc forming process according to claim 1, characterized in that: The air bag (500) is provided with an air nozzle (510), and the air nozzle (510) is connected to the outside. A through hole (610) for installing the air nozzle (510) is opened on one side of the upper mold, and the air nozzle (510) passes through the through hole (610).
9. The carbon fiber spoke disc forming process according to claim 1, characterized in that: The rough carbon fiber spoke disk (700) is formed on a carbon fiber spoke disk preforming jig, and the carbon fiber spoke disk (700) forming jig comprises a second lower mold (800), a second wedge block (810) and a second upper mold (820), wherein the second upper mold (820) is arranged directly above the second lower mold (800), and the second wedge block (810) is arranged between the second lower mold (800) and the second upper mold (820); a third forming surface (801) is provided on the upper surface of the second lower mold (800), and a hole forming column (802) is provided in the middle of the upper surface of the second lower mold (800); a fourth forming surface is provided on the lower surface of the second wedge block (810), and a fifth forming surface (811) is provided on the upper surface of the second wedge block (810); a first plug hole is provided in the middle of the lower surface of the second upper mold (820), and the hole forming column (802) cooperates with the first plug hole.
10. The carbon fiber spoke disc forming process according to claim 1, characterized in that: The rough blank of the carbon fiber spoke disk (700) comprises: a disk body made of carbon fiber material, a mounting hole (730) is opened in the middle of the disk body, the outer periphery of the disk body is composed of a first carbon fiber sheet (710) and a second carbon fiber sheet (720), an installation space for embedding spokes is formed between the first carbon fiber sheet (710) and the second carbon fiber sheet (720), the installation space comprises a first embedding groove (701) and a second embedding groove (702), the first embedding groove (701) and the second embedding groove (702) are alternately arranged along the circumference of the disk body, and the width e of the second embedding groove (702) is greater than the width f of the first embedding groove (701).
11. The carbon fiber spoke disc forming process according to claim 1, characterized in that: In step S1, preforming of the rough carbon fiber spoke disc (700) includes the following steps: b1, laying carbon yarn on the third molding surface (801) of the second lower mold (800) to form a first fiber sheet of the carbon fiber spoke disk (700); b2. Installing the second wedge block (810) on the first fiber sheet of the carbon fiber spoke disk (700) so that the upper surface of the first fiber sheet of the carbon fiber spoke disk (700) is in contact with the fourth molding surface; b3, laying carbon yarn on the fifth molding surface (811) to form a second fiber sheet of the carbon fiber spoke disk (700), wherein one side of the second fiber sheet is fixedly connected to the first fiber sheet and the other side is separated from the first fiber sheet, so that an installation space is formed between the first fiber sheet and the second fiber sheet; b4, installing the second upper mold (820) on the top of the second fiber sheet to fix the carbon yarn wound in the jig; b5. After fixing for a period of time, the mold is disassembled to obtain a rough blank of the carbon fiber spoke disc (700).
12. The carbon fiber spoke disc forming process according to claim 1, characterized in that: In step b5, the carbon yarn is fixed in the carbon fiber spoke disc preforming jig for half an hour.