Cold package method for rubber coating repair of belt conveyor roller
Through the cold packaging method of temperature and humidity control between glue wraps, the low production efficiency problem caused by glue wrapping or wear of the drum transporter is solved, and efficient rubber bonding and roller repair is achieved. It is suitable for various types of belt rollers. .
Patent Information
- Application Number
- CN202411163962.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the glue-covered or worn by the drum transporter leads to low production efficiency, and the on-site treatment method has problems such as poor environmental conditions, long construction time, high cost and limited applicability.
The cold-packing method is adopted, including pretreatment of the roller surface, applying glue, bonding rubber, and controlling the temperature and humidity between the glue, and conducting detection tests of dynamic balance, static balance, bonding strength, shear strength and peeling strength .
It effectively improves bonding strength, shortens repair time, reduces production costs, improves drum service life, and is suitable for belt rollers of different models and environments.
Smart Images

Figure CN118927681A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of roller rubber lagging repair, and in particular to a cold lagging method for repairing a belt conveyor roller rubber lagging. Background Art
[0002] Roller conveyors are currently widely used transportation machinery, especially for production and transportation systems consisting of multiple roller conveyors connected front and back. Each roller conveyor is a bottleneck. As long as one of them stops running due to a malfunction, it will inevitably cause the production enterprise to stop production and maintenance, which will squeeze the space for completing the task. Moreover, the longer the shutdown and maintenance time, the greater the economic loss.
[0003] In the actual operation of roller conveyors, the rubber coating of the rollers often becomes debonded or severely worn. If the rollers are not replaced or the rubber coating is not processed in time, the belts will seriously deviate, affecting the normal production. Serious accidents such as belt tearing may even occur, leading to production suspension and causing huge economic losses to the manufacturing company.
[0004] At present, there are many methods for on-site treatment of the wear of the rubber coating of the belt conveyor roller. Commonly used methods: one is to place a rubber-wrapped roller on site for each equipment as a spare. When the rubber coating of the used roller is degummed or severely worn, the production is stopped and the spare roller is replaced. Then the replaced roller is transported to the ground for rubber coating treatment, and then transported to the site as a spare after the treatment. The disadvantages of this method are poor on-site environmental conditions, long time to replace the spare roller, long idle time of the spare roller, resulting in high production costs, and high costs for transporting the roller back and forth. Especially when there are many belt conveyor equipment and different models, a large number of spare rollers lead to high production costs. Another method is to rubberize the roller on site, that is, first manually remove the original rubber coating on the roller, grind it, apply adhesive, and then bond the prepared rubber sheet to the roller. After bonding, it must be placed for a certain period of time to reach the bonding strength before it can be operated. The disadvantage of this method is that the construction time is long, and for humid construction sites (such as coal mines), due to factors such as dust, temperature, and moisture of the adhesive, it is easy to cause poor bonding quality and degumming. The third method is on-site integral casting, that is, after on-site grinding, the casting mold is set up, the raw materials are melted, cast, vulcanized (the vulcanization process alone takes more than 10 hours), cooled, and placed for a certain period of time to reach the bonding strength before the equipment can be restored to the operating state. This method requires a dry on-site environment, many tools and materials, a lot of labor, a long construction time, and a long production impact. Moreover, this method is only suitable for ground environments and not underground. Summary of the invention
[0005] In view of the shortcomings of the prior art described above, the object of the present invention is to provide a cold-wrapping method for repairing the rubber lagging of a belt conveyor roller, which is used to solve the problem in the prior art that the rubber lagging process of the roller has a great impact on the production efficiency when the rubber lagging of the roller conveyor is degummed or severely worn.
[0006] To achieve the above-mentioned purpose and other related purposes, the present invention provides a cold-wrapping method for repairing the rubber lagging of a belt conveyor roller, comprising the following steps:
[0007] S1: pre-treat the roller surface;
[0008] S2: Apply glue on the roller surface;
[0009] S3: bonding the rubber to the rubber coating layer on the roller surface in step S2;
[0010] S4: Conduct inspection test on the roller after the rubber is bonded.
[0011] Preferably, step S1 includes the following steps:
[0012] S1.1: Remove the worn rubber from the roller surface;
[0013] S1.2: Turn the roller surface to remove fatigue layer and rust;
[0014] S1.3: Perform flaw detection on the roller surface after turning in step S1.2;
[0015] S1.4: Clean the roller surface.
[0016] Preferably, in step S1.3, the roller surface after turning is subjected to flaw detection; when no defects are detected on the roller surface, step S1.4 is performed; when defects are detected on the roller surface, the roller surface is repaired; after the repair is completed, step S1.4 is performed.
[0017] Preferably, step S2 includes the following steps:
[0018] S2.1: Mix glue and curing agent in a ratio of 100:4 and stir evenly to form a mixed glue coating liquid;
[0019] S2.2: Brush the mixed glue coating liquid stirred evenly in step S2.1 evenly onto the roller surface, wait for it to solidify naturally to form a first glue coating layer; brush a second layer of mixed glue coating liquid on the first glue coating layer again, and then proceed to step S3.
[0020] Preferably, step S3 includes the following steps:
[0021] S3.1: Wrap the rubber on the roller surface, and use the rolling tool to roll the rubber back and forth to remove the bubbles in the bonding surface to ensure that the rubber fits the roller surface;
[0022] S3.2: Cut a V-shape at the rubber joint and polish it with a steel wire brush to clean the rubber powder and debris in the joint; fill it with mixed joint adhesive and compact it while filling; finally, polish it flat with a tungsten steel grinding butterfly;
[0023] S3.3: Cut off the excess rubber at both ends of the roller surface, and then apply a layer of cold vulcanizer on the edges of the rubber at both ends of the roller surface.
[0024] Preferably, the mixed joint adhesive in step S3.2 is glue, curing agent and rubber powder mixed in a ratio of 100:4:50 and stirred evenly.
[0025] Preferably, the detection tests performed in step S4 include a dynamic balance test, a static balance test, an adhesive strength test, a shear strength test, and a peel strength test.
[0026] Preferably, the requirement for the dynamic balance test is ≤0.020Nm (27.2g); the requirement for the static balance test is ≤0.250Nm (38.5g); the requirement for the bonding strength test is 3-4 (Pa.s); the requirement for the shear strength test is >2.2 (Mpa); and the requirement for the peel strength test is >100 (N / 2.5cm).
[0027] Preferably, the roller surface is pretreated in step S1, wherein the process of cleaning the roller surface is carried out in the rubber lagging room; the process of coating the roller surface with glue in step S2 and the process of bonding the rubber to the rubber coating layer on the roller surface in step S3 are both carried out in the rubber lagging room.
[0028] Preferably, the encapsulation room has temperature and humidity control functions, as well as dust removal functions; the temperature in the encapsulation room is controlled between 15° C. and 30° C., and the humidity is controlled between 60% and 75%.
[0029] As described above, the cold packing method for repairing the belt conveyor roller rubber lagging according to the present invention has the following beneficial effects:
[0030] 1. The cold packing method for repairing the belt conveyor roller lagging of the present invention is provided with a lagging room, and the temperature and humidity in the lagging room can be controlled, wherein the temperature is controlled between 15°C and 30°C, the humidity is controlled between 60% and 75%, and the thickness of the glue is controlled at 0.08mm, so that the curing time of the mixed glue liquid is about 15 minutes, which saves the repair time compared with the curing time of 30 minutes of the mixed glue liquid in other temperature and humidity environments. At the same time, the bonding strength of the mixed glue liquid can be effectively controlled in the temperature and humidity environment of the lagging room, and finally the bonding strength of the rubber can be guaranteed to be 3.6Pa.s and the peel strength is 145 (N / 2.5cm).
[0031] 2. The cold packing method for the belt conveyor roller lagging repair of the present invention improves the bonding strength, sorts out the entire cold packing technology to form a standardized operation, and reduces the quality risk. The lagging room is equipped with corresponding equipment to achieve a dust-free, temperature and humidity controllable environment, effectively control the solidification speed of the mixed glue coating liquid, reduce environmental pollution, and increase the service life of the belt conveyor roller, so as to achieve the purpose of reducing costs and increasing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a flow chart of a cold-wrapping method for repairing a belt conveyor roller by lagging. DETAILED DESCRIPTION
[0033] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0034] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change of the proportional relationship or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. The change or adjustment of their relative relationship should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.
[0035] like Figure 1 As shown, the present invention provides a cold packing method for repairing the rubber lagging of a belt conveyor roller, comprising the following steps:
[0036] S1: pre-treat the roller surface;
[0037] S1.1: Remove the worn rubber from the roller surface;
[0038] S1.2: Turning the roller surface to remove fatigue layer and rust; in this embodiment, turning makes the roller surface roughness>25≤50, so that the film will be more secure when bonding; the diameter φ of the roller surface after turning meets the technical requirements;
[0039] S1.3: Perform flaw detection on the roller surface after turning in step S1.2; when no defects are detected on the roller surface, proceed to step S1.4; when defects are detected on the roller surface, repair the roller surface; after the repair is completed, proceed to step S1.4. In this embodiment, the defects on the roller surface may be pits or the diameter does not meet the standard. In this case, welding repair can be performed on the pits or the outer periphery of the roller surface, and then the weld can be polished and repaired, so as to replace the roller skin of the roller surface;
[0040] S1.4: Clean the roller surface; in this embodiment, the roller surface is cleaned with a special cleaning agent and cleaned twice to thoroughly remove impurities such as oil, grease, dust, etc. on the surface of the roller that affect the bonding strength, and this step S1.4 is performed in a specially made lagging room.
[0041] S2: Apply glue on the roller surface;
[0042] S2.1: Mix the glue and curing agent in a ratio of 100:4, and stir evenly to form a mixed glue coating liquid; in this embodiment, the composition of the glue is a mixture of chloroprene film, resin, and solvent. Mix the glue and curing agent in a ratio of 100:4, and stir in one direction for three minutes with a stainless steel rod to completely mix them. Operators need to wear masks and gloves throughout the process;
[0043] S2.2: Apply the mixed glue solution stirred evenly in step S2.1 evenly onto the roller surface, wait for it to solidify naturally to form a first layer of glue; apply a second layer of mixed glue solution on the first layer of glue, and then proceed to step S3. In this embodiment, the natural solidification time of the first layer of glue is about 15 minutes, and the rubber bonding operation of step S3 is immediately performed after the second layer of mixed glue solution is applied on the first layer of glue, and the rubber bonding operation needs to be completed within 15 minutes to prevent the second layer of mixed glue solution from losing viscosity after solidification;
[0044] S3: bonding the rubber to the rubber coating layer on the roller surface in step S2;
[0045] S3.1: Wrap the rubber on the roller surface. The rubber bonding process should be carried out step by step. Use the rolling tool to roll the rubber back and forth to remove the bubbles in the bonding surface to ensure that the rubber fits the roller surface.
[0046] S3.2: Cut a V-shape at the rubber joint, and use a single steel wire brush to polish it to clean the rubber powder and debris in the joint; use a mixed joint adhesive to fill it, and compact it while filling; finally, use a tungsten steel polishing butterfly to polish it flat; in this embodiment, the mixed joint adhesive is a mixture of glue, curing agent and rubber powder in a ratio of 100:4:50, and stir it evenly.
[0047] S3.3: Cut off the excess rubber at both ends of the roller surface to form a 45° angle, and then brush a layer of cold vulcanizer on the edges of both ends of the roller surface;
[0048] S4: Perform a detection test on the roller after the rubber is bonded; in this embodiment, the detection tests performed on the roller include a dynamic balance test, a static balance test, a bonding strength test, a shear strength test, and a peel strength test; wherein, the dynamic balance test requirement is ≤0.020Nm (27.2g); the static balance test requirement is ≤0.250Nm (38.5g); the bonding strength test requirement is 3-4 (Pa.s); the shear strength test requirement is >2.2 (Mpa); the peel strength test requirement is >100 (N / 2.5cm).
[0049] Preferably, in this embodiment, the processes of cleaning the roller surface in step S1.4, applying glue on the roller surface in step S2, and bonding rubber to the glue layer on the roller surface in step S3 are all carried out in the rubber lagging room.
[0050] Preferably, the glue encapsulation room has temperature and humidity control functions, as well as dust removal functions; the temperature in the glue encapsulation room is controlled between 15°C-30°C, and the humidity is controlled between 60%-75%; the above temperature parameters and humidity parameters are the optimal curing state of the glue.
[0051] Preferably, in step S2.2, the thickness of the first coating layer and the second coating layer is controlled at 0.08 mm.
[0052] Preferably, the rolling tool used in step S3.1 can adopt a paper box laminating device with announcement number CN217099095U, and the laminating roller device in the above patent is changed to the roller in the present application, and a rotational force is applied to the roller, and the rubber on the roller surface of the roller is squeezed by relying on the rolling cylinder device above the roller to ensure the bonding strength of the rubber on the roller surface.
[0053] Preferably, in step S4, the dynamic balance test, static balance test, bonding strength test, shear strength test, and peel strength test are all performed on the test adhesive, and the test adhesive is made by the same operation as the roller surface lamination in the present application, and the destructive test is performed using the test adhesive.
[0054] The cold packing method for repairing the belt conveyor roller rubber packing according to the present invention has the following beneficial effects:
[0055] 1. The cold-packing method for rubber-packing repair of belt conveyor pulleys involved in the present invention is different from the hot-packing rubber-packing repair technology used in the prior art, which avoids serious pollution to the environment and is highly environmentally friendly.
[0056] 2. The present invention is specially made with a rubber lagging room, which can accurately control the temperature and humidity in the rubber lagging room. The entire rubber lagging process is carried out in the rubber lagging room, which effectively controls the speed of glue solidification and improves the bonding strength of the glue, thereby forming standardized operations, improving the bonding quality of the rubber on the roller surface, and extending the service life of the belt conveyor roller.
[0057] 3. The cold-wrapping method for repairing the belt conveyor pulley lagging involved in the present invention is that the entire lagging process is carried out in the lagging room. The curing time of the glue is controlled within 15 minutes by controlling the temperature and humidity. In this way, the lagging repair can be completed within 30 minutes. Compared with the prior art in which the curing time of a single layer of glue coating is 30 minutes, the repair time is saved and the repair efficiency can be effectively improved.
[0058] 4. The cold packing method for repairing the belt conveyor roller with rubber lagging involved in the present invention is suitable for belt conveyor rollers of φ300-φ2000. The length of the roller is not limited, the application range is wide, and it is easy to promote.
[0059] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.
[0060] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A cold packing method for repairing belt conveyor roller lagging, characterized in that: The steps include: S1: pre-treat the roller surface; S2: Apply glue on the roller surface; S3: bonding the rubber to the rubber coating layer on the roller surface in step S2; S4: Conduct inspection test on the roller after the rubber is bonded.
2. The cold packing method for repairing the belt conveyor roller lagging according to claim 1 is characterized in that: Step S1 includes the following steps: S1.1: Remove the worn rubber from the roller surface; S1.2: Turn the roller surface to remove fatigue layer and rust; S1.3: Perform flaw detection on the roller surface after turning in step S1.2; S1.4: Clean the roller surface.
3. The cold packing method for repairing the belt conveyor roller lagging according to claim 2 is characterized in that: In step S1.3, flaw detection is performed on the roller surface after turning; when no defects are detected on the roller surface, step S1.4 is performed; when defects are detected on the roller surface, the roller surface is repaired; after the repair is completed, step S1.4 is performed.
4. The cold packing method for repairing the belt conveyor roller lagging according to claim 1 is characterized in that: Step S2 includes the following steps: S2.1: Mix glue and curing agent in a ratio of 100:4 and stir evenly to form a mixed glue coating liquid; S2.2: Brush the mixed glue coating liquid stirred evenly in step S2.1 evenly onto the roller surface, wait for it to solidify naturally to form a first glue coating layer; brush a second layer of mixed glue coating liquid on the first glue coating layer again, and then proceed to step S3.
5. The cold packing method for repairing the belt conveyor roller lagging according to claim 1 is characterized in that: Step S3 includes the following steps: S3.1: Wrap the rubber on the roller surface, and use the rolling tool to roll the rubber back and forth to remove the bubbles in the bonding surface to ensure that the rubber fits the roller surface; S3.2: Cut a V-shape at the rubber joint and polish it with a steel wire brush to clean the rubber powder and debris in the joint; fill it with mixed joint adhesive and compact it while filling; finally, polish it flat with a tungsten steel grinding butterfly; S3.3: Cut off the excess rubber at both ends of the roller surface, and then apply a layer of cold vulcanizer on the edges of the rubber at both ends of the roller surface.
6. The cold-packing method for repairing the belt conveyor roller lagging according to claim 5 is characterized in that: The mixed joint adhesive in step S3.2 is a mixture of glue, curing agent and rubber powder in a ratio of 100:4:50, and stirred evenly.
7. The cold-packing method for repairing the belt conveyor roller lagging according to claim 1 is characterized in that: The detection tests performed in step S4 include a dynamic balance test, a static balance test, an adhesive strength test, a shear strength test, and a peel strength test.
8. The cold-packing method for repairing the belt conveyor roller lagging according to claim 7 is characterized in that: The requirement for the dynamic balance test is ≤0.020Nm (27.2g); the requirement for the static balance test is ≤0.250Nm (38.5g); the requirement for the bonding strength test is 3-4 (Pa.s); the requirement for the shear strength test is >2.2 (Mpa); and the requirement for the peel strength test is >100 (N / 2.5cm).
9. The cold-packing method for repairing the belt conveyor roller lagging according to claim 1 is characterized in that: In step S1, the roller surface is pretreated, wherein the process of cleaning the roller surface is carried out in the rubber lagging room; in step S2, the process of coating the roller surface with glue and in step S3, the process of bonding the rubber to the coating layer on the roller surface are both carried out in the rubber lagging room.
10. The cold-wrapping method for repairing the belt conveyor roller lagging according to claim 9 is characterized in that: The rubber coating room has temperature and humidity control functions and dust removal functions; the temperature in the rubber coating room is controlled between 15° C. and 30° C., and the humidity is controlled between 60% and 75%.