Manufacturing method of rubber hose
By using polyurethane rubber and neoprene combined with silica and wire braided layer, a high-strength rubber hose is formed, which solves the problem of existing rubber hoses being easily deformed or broken under high pressure, and improves their pressure bearing capacity and Service life.
Patent Information
- Application Number
- CN202411314966.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
AI Technical Summary
Existing rubber hoses are prone to deformation or breakage when subjected to high pressure, resulting in their inability to meet the requirements of high pressure applications and have a short service life.
Polyurethane rubber and neoprene are used as base glue and reinforcement glue, combined with silica and wire braiding layer, the inner and outer glue layer is formed through a double-roll mill and an extruder, and the steel wire reinforcement layer is woven on the braiding machine. , and finally the vulcanization treatment is carried out in the vulcanizer, controlling the temperature and tension to ensure uniform adhesion and bonding.
It improves the overall strength and pressure resistance of the rubber hose, reduces the possibility of deformation or rupture, and extends the service life.
Smart Images

Figure CN118927688A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber hose manufacturing, and in particular to a rubber hose manufacturing method. Background Art
[0002] Rubber hose is a highly flexible pipe that can be easily bent to adapt to various complex installation environments. Rubber hose is usually composed of an inner rubber layer, a reinforcement layer (such as a steel wire braided layer or a fiber braided layer) and an outer rubber layer. The inner rubber layer is in direct contact with the fluid; the reinforcement layer is used to improve the pressure bearing capacity of the hose, and is often made of steel wire braiding or winding; the outer rubber layer plays a protective role to prevent the external environment from causing damage to the hose;
[0003] At present, rubber hoses are widely used in the fields of petroleum, chemical industry, shipbuilding, irrigation, fire fighting, etc. to transport various liquids, gases and solid particles. For example, in agricultural irrigation, rubber hoses can be used to transport water; in industrial production, they can be used to transport oil, chemicals, etc.; but the manufacturing methods of most rubber hoses are not perfect, resulting in insufficient strength of the produced rubber hoses. They are prone to deformation or cracking and breaking when subjected to high pressure, resulting in their inability to meet the requirements of certain high-pressure applications. There are certain usage defects and the service life of the rubber hoses is shortened. Summary of the invention
[0004] To this end, the present invention provides a method for manufacturing a rubber hose to solve the above-mentioned problems in the prior art.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] According to a first aspect of the present invention, a method for manufacturing a rubber hose is provided, and the specific implementation steps are as follows:
[0007] S1: weigh 150-200 parts of polyurethane rubber, 75-100 parts of chloroprene rubber, 20-40 parts of silicon dioxide, 5-8 parts of vulcanizing agent, 1-3 parts of lauric acid, 2-5 parts of zinc oxide, 0.5-1.5 parts of accelerator, and 0.5-1.5 parts of ultraviolet absorber;
[0008] S2: Add polyurethane rubber and chloroprene rubber to a double-roll mill and plasticize for 5-8 minutes, then add lauric acid, zinc oxide, accelerator and ultraviolet absorber in sequence, adjust the temperature of the double-roll mill to 65-75°C, mix for 5-10 minutes, then add 20-30 parts of reinforcement cloth, mix for 5-10 minutes, add silica and vulcanizing agent at the end of mixing, mix evenly, and obtain a mixed rubber;
[0009] S3: Put the rubber compound into the hopper of the extruder, adjust the temperature of the extruder between 70-120℃, and the extrusion time is 5-15 minutes. The rubber compound is heated and extruded by the extruder, gradually softened, pushed into the die head, extruded through the extrusion hole of the die to form an inner rubber layer, and the inner rubber layer is cooled by the cooling equipment;
[0010] S4: Fix the inner rubber hose on the fixture of the braiding machine, and use the braiding machine to continuously braid the steel wire on the outside of the inner rubber layer to form a reinforcement layer. The braiding temperature should be maintained between 35-100℃, and the tension should be controlled in the range of 2-20N / bundle;
[0011] S5: the mixed rubber in S2 is put into the hopper of the extruder again, and the mixed rubber is extruded through the extruder and the extrusion hole of the die to form a continuous outer rubber layer, which is tightly coated on the outside of the inner rubber layer and the reinforcement layer to form a hose;
[0012] S6: Put the hose into a vulcanizer for vulcanization treatment, control the vulcanization temperature at 150-200°C, and vulcanize for 1-1.5 hours at a pressure of 0.3-0.8MPa to obtain a finished rubber hose.
[0013] Furthermore, the cooling time of the cooling device is 20-40 minutes, and the cooling temperature is between 30-60°C.
[0014] Furthermore, the reinforcement cloth needs to be cleaned 2-3 times before adding, and needs to be dried at a constant temperature of 60°C after cleaning.
[0015] Furthermore, the temperature of the extruder in S5 is controlled between 60-110° C., the extrusion time is 5-15 minutes, and the extrusion temperature of the outer rubber layer is lower than the extrusion temperature of the inner rubber layer.
[0016] Furthermore, the reinforcement cloth is one or more of glass fiber cloth, carbon fiber cloth or aramid fiber cloth.
[0017] Furthermore, the polyurethane rubber is the base rubber, the chloroprene rubber is the reinforcing rubber, and the silicon dioxide is the filling and reinforcing agent.
[0018] The present invention has the following advantages:
[0019] 1. The weaving temperature should be kept between 35-100℃ during weaving to avoid excessive temperature causing material performance degradation. At the same time, the tension should be controlled within the range of 2-20N / beam to ensure that the reinforcement layer can be evenly attached to the inner rubber layer to improve the overall strength and pressure resistance;
[0020] 2. The overall strength is enhanced by using one or more of the reinforcement cloth, such as glass fiber cloth, carbon fiber cloth or aramid fiber cloth, and combining it with a reinforcement layer evenly attached to the inner rubber layer. This can improve the ability of the finished rubber hose to withstand high pressure and reduce the possibility of deformation or rupture. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A flow chart of a method for manufacturing a rubber hose provided in some embodiments of the present invention. DETAILED DESCRIPTION
[0022] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] like Figure 1 As shown, a method for manufacturing a rubber hose in an embodiment of the first aspect of the present invention uses polyurethane rubber as a base rubber, chloroprene rubber as a reinforcing rubber, and silicon dioxide as a filling and reinforcing agent. The specific implementation steps are as follows:
[0025] S1: Weigh 150 parts of polyurethane rubber, 100 parts of chloroprene rubber, 20 parts of silicon dioxide, 5 parts of vulcanizing agent, 1 part of lauric acid, 5 parts of zinc oxide, 0.5 parts of accelerator, and 1.5 parts of ultraviolet absorber by weight;
[0026] S2: polyurethane rubber and chloroprene rubber are added to a two-roll mill and plasticized for 8 minutes, and then lauric acid, zinc oxide, accelerator and ultraviolet absorber are added in sequence, the temperature of the two-roll mill is adjusted to 75°C, and mixed for 10 minutes, and then 20 parts of reinforcement cloth are added and mixed for 10 minutes. Silica and vulcanizing agent are added in the later stage of mixing to ensure full mixing and uniform dispersion, and the mixing is uniform to obtain a mixed rubber, which can increase the temperature of the rubber compound and increase the thermoplasticity;
[0027] S3: Put the rubber compound into the hopper of the extruder, adjust the temperature of the extruder to 70°C, and the extrusion time is 5 minutes. The rubber compound is heated and extruded by the extruder, gradually softened, pushed into the die head, and extruded through the extrusion hole of the die to form an inner rubber layer. The inner rubber layer is cooled by a cooling device. The cooling time is 20 minutes, and the cooling temperature is between 30-60°C, so that the inner rubber layer is gradually cooled and solidified;
[0028] S4: Fix the inner rubber hose on the clamp of the braiding machine, and use the braiding machine to continuously braid the steel wire on the outside of the inner rubber layer to form a reinforcement layer. The braiding temperature should be kept between 35℃ to avoid excessive temperature causing material performance degradation. At the same time, the tension range should be controlled within 20N / bundle to ensure that the reinforcement layer can be evenly attached to the inner rubber layer to improve the overall strength and pressure resistance;
[0029] S5: The mixed rubber in S2 is put into the hopper of the extruder again, and the mixed rubber is extruded through the extruder and the extrusion hole of the die to form a continuous outer rubber layer, which is tightly coated on the outside of the inner rubber layer and the reinforcement layer to form a hose. The temperature of the extruder is controlled between 60-110°C, and the extrusion time is 5-15 minutes. The extrusion temperature of the outer rubber layer is lower than that of the inner rubber layer, so that the outer rubber layer can form good adhesion with the inner rubber layer and the reinforcement layer;
[0030] S6: Put the hose into a vulcanizer for vulcanization treatment, control the vulcanization temperature at 150°C, and vulcanize for 1.5 hours at a pressure of 0.8 MPa to obtain a finished rubber hose;
[0031] Lauric acid is conducive to the full diffusion of silicon dioxide in polyurethane rubber and can promote its activity. At the same time, zinc oxide and lauric acid can be used together to generate soluble zinc salts. The accelerator acts to form a complex with good solubility in rubber, activates the accelerator and sulfur, and improves the vulcanization efficiency. The accelerator can accelerate the vulcanization reaction, improve production efficiency, and ensure the uniformity of the vulcanization process. The ultraviolet absorber can absorb ultraviolet rays to prevent its destructive effect on rubber and extend the service life of the hose in outdoor environments.
[0032] The reinforcement cloth is one or more of glass fiber cloth, carbon fiber cloth or aramid fiber cloth. The reinforcement cloth needs to be cleaned 2-3 times before adding. After cleaning, it needs to be dried at a constant temperature of 60°C to ensure its cleanliness and dryness, which helps to improve the bonding force between the reinforcement cloth and the rubber material. Mixing can ensure that the reinforcement cloth is evenly distributed in the mixed rubber to avoid aggregation or stratification, thereby improving the overall angle of the rubber hose. At the same time, the reinforcement layer evenly attached to the inner rubber layer can enhance the overall strength, which can improve the ability of the finished rubber hose to withstand high pressure and reduce the possibility of deformation or cracking;
[0033] Example 2
[0034] A method for manufacturing a rubber hose comprises the following steps:
[0035] S1: Weigh 200 parts of polyurethane rubber, 80 parts of chloroprene rubber, 40 parts of silicon dioxide, 6 parts of vulcanizing agent, 3 parts of lauric acid, 5 parts of zinc oxide, 1.5 parts of accelerator, and 1 part of ultraviolet absorber by weight;
[0036] S2: polyurethane rubber and chloroprene rubber are added to a two-roll mill and plasticized for 5 minutes, and then lauric acid, zinc oxide, accelerator and ultraviolet absorber are added in sequence, the temperature of the two-roll mill is adjusted to 70° C., and mixed for 5 minutes, and then 30 parts of reinforcement cloth are added, and mixed for 10 minutes. Silica and vulcanizing agent are added at the end of mixing, and the materials are mixed evenly to obtain a mixed rubber;
[0037] S3: Put the rubber compound into the hopper of the extruder, adjust the temperature of the extruder to 120°C, and the extrusion time is 15 minutes. The rubber compound is heated and extruded by the extruder, gradually softened, pushed into the die head, extruded through the extrusion hole of the die to form an inner rubber layer, and the inner rubber layer is cooled by the cooling equipment;
[0038] S4: Fix the inner rubber hose on the fixture of the braiding machine, and use the braiding machine to continuously braid the steel wire on the outside of the inner rubber layer to form a reinforcement layer. The braiding temperature should be maintained at 100℃, and the tension should be controlled within 15N / bundle;
[0039] S5: the mixed rubber in S2 is put into the hopper of the extruder again, and the mixed rubber is extruded through the extruder and the extrusion hole of the die to form a continuous outer rubber layer, which is tightly coated on the outside of the inner rubber layer and the reinforcement layer to form a hose;
[0040] S6: Put the hose into a vulcanizer for vulcanization treatment, control the vulcanization temperature at 200°C, and vulcanize at a pressure of 0.5 MPa for 1 hour to obtain a finished rubber hose.
[0041] It should be understood that these embodiments are only to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention.
Claims
1. A method for manufacturing a rubber hose, characterized in that: The specific implementation steps are as follows: S1: weigh 150-200 parts of polyurethane rubber, 75-100 parts of chloroprene rubber, 20-40 parts of silicon dioxide, 5-8 parts of vulcanizing agent, 1-3 parts of lauric acid, 2-5 parts of zinc oxide, 0.5-1.5 parts of accelerator, and 0.5-1.5 parts of ultraviolet absorber; S2: Add polyurethane rubber and chloroprene rubber to a double-roll mill and plasticize for 5-8 minutes, then add lauric acid, zinc oxide, accelerator and ultraviolet absorber in sequence, adjust the temperature of the double-roll mill to 65-75°C, mix for 5-10 minutes, then add 20-30 parts of reinforcement cloth, mix for 5-10 minutes, add silica and vulcanizing agent at the end of mixing, mix evenly, and obtain a mixed rubber; S3: Put the rubber compound into the hopper of the extruder, adjust the temperature of the extruder between 70-120℃, and the extrusion time is 5-15 minutes. The rubber compound is heated and extruded by the extruder, gradually softened, pushed into the die head, extruded through the extrusion hole of the die to form an inner rubber layer, and the inner rubber layer is cooled by the cooling equipment; S4: Fix the inner rubber hose on the fixture of the braiding machine, and use the braiding machine to continuously braid the steel wire on the outside of the inner rubber layer to form a reinforcement layer. The braiding temperature should be maintained between 35-100℃, and the tension should be controlled in the range of 2-20N / bundle; S5: the mixed rubber in S2 is put into the hopper of the extruder again, and the mixed rubber is extruded through the extruder and the extrusion hole of the die to form a continuous outer rubber layer, which is tightly coated on the outside of the inner rubber layer and the reinforcement layer to form a hose; S6: Put the hose into a vulcanizer for vulcanization treatment, control the vulcanization temperature at 150-200°C, and vulcanize for 1-1.5 hours at a pressure of 0.3-0.8MPa to obtain a finished rubber hose.
2. A method for manufacturing a rubber hose according to claim 1, characterized in that: The cooling time of the cooling device is 20-40 minutes, and the cooling temperature is between 30-60°C.
3. A method for manufacturing a rubber hose according to claim 1, characterized in that: The reinforcement cloth needs to be cleaned 2-3 times before adding, and needs to be dried at a constant temperature of 60°C after cleaning.
4. A method for manufacturing a rubber hose according to claim 1, characterized in that: The temperature of the extruder in S5 is controlled between 60-110° C., the extrusion time is 5-15 minutes, and the extrusion temperature of the outer rubber layer is lower than the extrusion temperature of the inner rubber layer.
5. The method for manufacturing a rubber hose according to claim 1, characterized in that: The reinforcement cloth is one or more of glass fiber cloth, carbon fiber cloth or aramid fiber cloth.
6. A method for manufacturing a rubber hose according to claim 5, characterized in that: The polyurethane rubber is the base rubber, the chloroprene rubber is the reinforcing rubber, and the silicon dioxide is the filling and reinforcing agent.