Lightweight melamine thermal insulation board and preparation method thereof
Through the hot pressing forming technology of modified melamine insulation resin and basalt fiber fabric, the problem of insufficient performance of heat insulation materials in the existing technology was solved, and high-performance, lightweight, thin-layer melamine insulation boards were prepared, suitable for new Energy vehicles and lithium battery packs and other fields.
Patent Information
- Application Number
- CN202410978062.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The prior art is difficult to meet the demands of modern transportation, building insulation and energy industries for high-performance, lightweight, thin-layer sandwich insulation materials, especially in terms of safety, mechanical strength, flame retardancy and environmental protection.
Light melamine insulation panels are prepared by hot pressing the multi-layer overlapping modified melamine thermal insulation resin fiber fabric. The modified melamine thermal insulation resin adhesive is used to combine with basalt fiber fabric, containing melamine resin, silicone resin, poly Ether-modified epoxy resin and nanomodifier are composed of excellent insulation, flame retardant and mechanical properties.
The density was prepared from 1.52g/cm3 to 1.75g/cm3, the thermal conductivity was less than 0.2w/m·k, the bending strength was 350MPa to 420MPa, the tensile strength was 336MPa to 372MPa, and the notch impact strength was 65KJ/m2 to 75KJ/m2. Lightweight melamine insulation board with insulation resistance greater than 108MΩ and flame retardancy reaches UL94 V-0 level, suitable for new energy vehicles and lithium battery packs and other fields.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The present invention belongs to laminated boards and their preparation, and relates to a lightweight melamine insulation board and its preparation method. The lightweight melamine insulation board of the present invention (prepared) is suitable for use in the fields of transportation, building insulation, energy industry, etc., and is particularly suitable for use as a lightweight insulation material in the fields of new energy vehicles, lithium battery packs, submarine pipeline transportation, etc. Background Art
[0002] With the technological development in fields such as 5G, big data, artificial intelligence, and the Internet of Things, the power density of electronic devices continues to rise, and efficient thermal management materials and solutions are urgently needed to ensure the efficiency, reliability, safety, durability, and continuous stability of products.
[0003] Thermal insulation material is a material or a composite of materials with insulating properties and shielding effect on heat flow. It is usually light, loose, porous, and has low thermal conductivity. It is widely used in industry to prevent heat loss in thermal equipment and pipelines, or used under freezing and low temperature conditions, so it is also called thermal insulation or cold insulation material. At the same time, due to its porous or fibrous structure with good sound absorption function, it is also widely used in the construction industry. Lightweight thermal insulation material is a new type of lightweight, efficient, energy-saving and environmentally friendly material. The widespread application of lightweight thermal insulation material will help reduce energy consumption, reduce environmental pollution, and improve economic and social benefits. It is widely used in transportation, building insulation, energy industry and other fields.
[0004] For power battery packs, thermal runaway is the main cause of safety accidents. Under high energy density, battery fire or explosion may occur due to battery batch consistency, thermal stability of the material itself, compatibility between battery components, and high flammability of the electrolyte. After a battery cell experiences thermal runaway, the battery system is required to be free of fire and explosion within 5 minutes. To achieve a "5-minute safe escape time", corresponding technical requirements are required for the thermal insulation materials of the battery pack to delay the explosion time of the faulty battery pack. As China's new energy vehicle market and energy storage lithium battery market continue to grow rapidly, the market demand for lithium battery thermal management flame-retardant insulation materials will show a blowout development trend.
[0005] In pursuit of volume energy density, lithium battery factories are designing battery packs with an increasingly intensive trend in terms of overall volume and weight. They have also put forward revolutionary requirements for the battery pack outer packaging partitions they use, requiring them to ensure that the battery pack is lightweight (low density), has high energy utilization (low thermal conductivity), and is highly safe (flame retardant). In addition, they are required to have excellent support strength, deformation resistance (mechanical strength), insulation performance (electrical strength), and thinner sheet thickness (can be greater than or equal to 0.5 mm). These are things that cannot be achieved by foam materials with low mechanical strength and large thickness in the prior art. The prior art is difficult to meet the needs of modern transportation, building insulation, energy industry and other fields for sandwich insulation materials with higher requirements for dimensional accuracy, mechanical and electrical strength, flame retardancy, and environmental protection. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a lightweight melamine insulation board and a preparation method thereof. 3 ~1.75g / cm 3 ), high thermal insulation (thermal conductivity (25°C) less than 0.2w / m·k), high strength (flexural strength of 350MPa~420MPa, tensile strength of 336MPa~372MPa), high heat resistance (flexural strength at 150°C 207MPa~266MPa), high toughness (notch impact strength of 65KJ / m 2 ~75KJ / m 2 ), excellent insulation (insulation resistance greater than or equal to 10 8 The invention discloses a lightweight melamine heat-insulating board with high thermal conductivity, low carbonization temperature and low heat release rate (MΩ), flame retardancy (reaching UL94 V-0 level) and thin board thickness (which can be greater than or equal to 0.5 mm) and a preparation method thereof.
[0007] The present invention provides a lightweight melamine insulation board, which is characterized in that the lightweight melamine insulation board is a lightweight melamine insulation board obtained by hot pressing multiple layers of overlapping modified melamine insulation resin fiber fabric prepreg (the number of layers of the modified melamine insulation resin fiber fabric prepreg is not limited, and can be 1-500 layers according to needs);
[0008] The modified melamine heat-insulating resin fiber fabric prepreg is obtained by coating the modified melamine heat-insulating resin adhesive on the basalt fiber fabric and then baking;
[0009] The modified melamine heat-insulating resin adhesive is composed of 100 parts by weight of melamine resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of polyether-modified epoxy resin, 5-25 parts by weight of melamine salt, 10-40 parts by weight of nano-modifier, 0.01-0.06 parts by weight of modification treatment agent, 0.2-13 parts by weight of curing agent, 0.005-0.1 parts by weight of accelerator and 60-400 parts by weight of solvent;
[0010] The basalt fiber fabric is at least one of basalt fiber plain fabric, basalt fiber twill fabric, basalt fiber gingham fabric, basalt fiber multi-axial fabric, and basalt fiber composite fabric (the production and provision companies and product models (brands) of the basalt fiber fabric include: Ningbo Fangtai Fiberglass Products Co., Ltd., Jiangsu Kangdafu New Materials Technology Co., Ltd., Tongxiang Lanshi Composite Materials Co., Ltd., etc.).
[0011] In the modified melamine thermal insulation resin adhesive in the content of the present invention:
[0012] The melamine resin is a highly etherified melamine formaldehyde resin [the production and supply enterprises and product models (brands) of the highly etherified melamine formaldehyde resin include: JY-303 of Jining Juyue New Materials Co., Ltd., CYMEL303LF of Allnex, etc.];
[0013] The polyether-modified epoxy resin is produced by: Japanese ADEKA's EP-1307, EP-4000, etc.
[0014] The organic silicone resin, the production and providing enterprises and product models (brands) of the organic silicone resin are: SI-101 of Laiyang Shengbang Organic Silicon Technology Co., Ltd., KR-271 of Shin-Etsu Chemical Co., Ltd. of Japan, SM1153D of Sanmu Group, etc.;
[0015] The melamine salt is phosphate [the production and provision of the phosphate include: Jinan Taizhong Kexing New Material Technology Co., Ltd., Guangzhou Shanghe Chemical Technology Co., Ltd.'s X2023, etc.], polyphosphate [the production and provision of the polyphosphate include: Hubei Longxin Chemical Industry Co., Ltd.'s LX9685, Zhongshan Dixin Chemical Co., Ltd.'s DBFPE, etc.], ammonium polyphosphate [the production and provision of the ammonium polyphosphate include: Guangzhou Yinyuan New Materials Co., Ltd. FR-AP1001 of Jinan Xinnuo Chemical Co., Ltd., APP of Jinan Haobang Chemical Co., Ltd., etc.], dimelamine pyrophosphate [the production and product models (brands) of the dimelamine pyrophosphate are: Senfida Chemical, Wuhan Huaxiang Kejie Biotechnology Co., Ltd., etc.], melamine cyanurate [the production and product models (brands) of the melamine cyanurate are: Guangzhou Yinyuan New Materials Co., Ltd., Shandong Qizhuo New Materials Technology Co., Ltd., etc.] any one or a mixture of two or more thereof;
[0016] The curing agent is a mixture of any two or more of diaminodiphenyl sulfone [the production and provision of diaminodiphenyl sulfone include: DDS of Jingmen Dongxin Biotechnology Co., Ltd., PA04296 of Guangdong Wengjiang Biotechnology Co., Ltd., etc.], dicyandiamide [the production and provision of dicyandiamide include: Jinan Kaichuang Chemical Co., Ltd., Guangzhou Xinxi Metallurgical Chemical Co., Ltd., etc.], and diaminodiphenylmethane [the production and provision of diaminodiphenylmethane include: Wuhan Zhisheng Technology Co., Ltd., Zhangjiagang Yarui Chemical Co., Ltd., Guangzhou Yangming Chemical Technology Co., Ltd., etc.];
[0017] The nano-modifier is one or a mixture of two of fumed silica [the fumed silica is produced by companies and product models (brands): TT 1000granulate of Suzhou Unocal Insulation Technology Co., Ltd.] and hollow glass microspheres [the hollow glass microspheres are produced by companies and product models (brands): C-40 of Zhongke Huaxing New Materials Co., Ltd., S4630 of 3M Company, etc.];
[0018] The modifying agent is any one of 3-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-aminopropyl triethoxysilane include: Shandong Tianming Biotechnology Development Co., Ltd., Shandong Xiya Chemical Co., Ltd., Linyi Azeroth Biotechnology Co., Ltd., etc.], 3-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-glycidyloxypropyl trimethoxysilane include: Hubei Yongkuo Technology Co., Ltd., Nantong Runfeng Petrochemical Co., Ltd., Guangdong Wengjiang Chemical Reagent Co., Ltd., etc.], γ-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-aminopropyl triethoxysilane include: Hangzhou Jessica Chemical Co., Ltd., Henan Wanshan New Materials Technology Co., Ltd., etc.], γ-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-glycidyloxypropyl trimethoxysilane include: Henan Xinpeng Chemical Products Co., Ltd., Henan Xiye Chemical Co., Ltd., etc.] or a mixture of two or more thereof;
[0019] The accelerator is any one of imidazole [the production and provision of the imidazole include: 2-methylimidazole of Linyi Mingpin Chemical Co., Ltd., N,N'-carbonyldiimidazole of Shanghai Nuotai Chemical Co., Ltd., etc.], acetyl metal complex [the production and provision of the acetyl metal complex include: No. 3 curing agent of Hubei Hongfuda Biotechnology Co., Ltd., etc.], boron trifluoride ethylamine [the production and provision of boron trifluoride ethylamine include: Beijing Xinao Xunchi Chemical Co., Ltd., Nanjing Chemical Reagent Co., Ltd., etc.], p-toluenesulfonic acid [the production and provision of p-toluenesulfonic acid include: Datang Chemical Co., Ltd., Ji Chuang Chemical Co., Ltd., Shandong Dongyue New Materials Technology Co., Ltd., etc.], methanesulfonic acid [the production and provision of methanesulfonic acid include: Langyu Chemical, Jinan Ronghui Chemical, etc.] or a mixture of two or more thereof;
[0020] The solvent is toluene [the toluene production and providing enterprises and product models (brands) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd., etc.], xylene [the xylene production and providing enterprises and product models (brands) include: Shandong Ruigang Chemical Co., Ltd., Shandong Guanyi Chemical Co., Ltd., etc.], acetone [the acetone production and providing enterprises and product models (brands) include: Jinan Daliang Chemical Co., Ltd., Kunshan Minglong Chemical Co., Ltd.], butanone [the butanone production and providing enterprises and product models (brands) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd. etc.], ethanol [the production and provision of ethanol and the product models (trademarks) include: Foshan Changxing New Materials Co., Ltd., Shandong Xinhongfeng New Materials Technology Co., Ltd., etc.], ethylene glycol methyl ether [the production and provision of ethylene glycol methyl ether and the product models (trademarks) include: Shandong Jinyueyuan New Materials Co., Ltd., Shandong Jinyueyuan New Materials Co., Ltd., etc.], N,N-dimethylformamide [the production and provision of N,N-dimethylformamide and the product models (trademarks) include: Dongguan Nanjian Fine Chemical Co., Ltd., Guangzhou Futuo Trading Co., Ltd., etc.] any one or a mixture of two or more thereof.
[0021] In the content of the present invention: the hot pressing molding is preferably: after preheating the template at 105°C to 155°C, the modified melamine insulation resin fiber fabric prepreg is overlapped (including matching and laminating) and placed in the template, and after the mold is closed, it is hot pressed at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa, and the hot pressing time is 0.5h to 50h (h means hours, the same below).
[0022] In the content of the present invention: the baking is preferably: putting the basalt fiber fabric coated with modified melamine thermal insulation resin adhesive (through a gluing machine) into a drying tunnel, the drying tunnel is 50m long, divided into 4 sections, each section is 12.5m, the baking temperature range is 75°C to 175°C, wherein: the first section is 75°C to 95°C, the second section is 105°C to 135°C, the third section is 135°C to 175°C, and the fourth section is 85°C to 110°C, and the speed of the gluing machine is 5m / min to 25m / min.
[0023] In the content of the present invention: the preparation method of the modified melamine thermal insulation resin adhesive is preferably: at a temperature of 50°C to 85°C, the nano modifier, the modification agent, the polyether modified epoxy resin and the silicone resin are stirred and mixed at a speed of 800r / min to 1500r / min, stirred for 1h to 3h (to prepare the modified resin for standby use), and then a curing agent is added and mixed and stirred at room temperature, and after stirring for 0.5h to 2.5h, melamine resin and melamine salt are added, and mixed and stirred at room temperature, and after stirring for 0.75h to 1.5h, a solvent and a accelerator are added, and after stirring and mixing at room temperature, the resin molding time is tested to be 320s to 450s at 160°C, and the modified melamine thermal insulation resin adhesive is obtained.
[0024] In the content of the present invention: in the modified melamine thermal insulation resin fiber fabric prepreg: the weight percentage of the (semi-cured) modified melamine thermal insulation resin adhesive is preferably 25% to 50%, and the weight percentage of the basalt fiber fabric is preferably 50% to 75%.
[0025] In the context of the present invention: the lightweight melamine insulation board has a light weight (density of 1.52g / cm 3 ~1.75g / cm 3 ), high thermal insulation (thermal conductivity (25°C) less than 0.2w / m·k), high strength (flexural strength of 350MPa~420MPa, tensile strength of 336MPa~372MPa), high heat resistance (flexural strength at 150°C 207MPa~266MPa), high toughness (notch impact strength of 65KJ / m 2 ~75KJ / m 2 ), excellent insulation (insulation resistance greater than or equal to 10 8 The invention discloses a lightweight melamine insulation board having the characteristics of high thermal conductivity, low carbonization temperature and low thermal conductivity, high thermal conductivity, low saturation and low thermal conductivity, and high thermal conductivity. The invention discloses a lightweight melamine insulation board having the characteristics of high thermal conductivity, ...
[0026] Another aspect of the present invention is: a method for preparing a lightweight melamine insulation board, which is characterized in that it comprises the following steps:
[0027] a. Ingredients: prepare the raw materials of each component according to the ratio of 100 parts by weight of melamine resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of polyether modified epoxy resin, 5-25 parts by weight of melamine salt, 10-40 parts by weight of nano modifier, 0.01-0.06 parts by weight of modification treatment agent, 0.2-13 parts by weight of curing agent, 0.005-0.1 parts by weight of accelerator and 60-400 parts by weight of solvent;
[0028] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 50° C. to 85° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin are stirred and mixed at a speed of 800 r / min to 1500 r / min, stirred for 1 h to 3 h (to prepare the modified resin for standby use), and then a curing agent is added and mixed and stirred at room temperature, and after stirring for 0.5 h to 2.5 h, melamine resin and melamine salt are added, and mixed and stirred at room temperature, and after stirring for 0.75 h to 1.5 h, a solvent and an accelerator are added, and after stirring and mixing at room temperature, the resin molding time is tested to be 320 s to 450 s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0029] c. Preparing a modified melamine thermal insulation resin fiber fabric prepreg: coating the modified melamine thermal insulation resin adhesive prepared in step b on the basalt fiber fabric, and then baking to obtain a modified melamine thermal insulation resin fiber fabric prepreg;
[0030] The basalt fiber fabric is at least one of basalt fiber plain fabric, basalt fiber twill fabric, basalt fiber woven fabric, basalt fiber multi-axial fabric, and basalt fiber composite fabric;
[0031] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, close the mold and perform hot pressing at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa for 0.5h to 50h to obtain a lightweight melamine insulation board.
[0032] In another aspect of the present invention: the baking is preferably to put the basalt fiber fabric coated with modified melamine thermal insulation resin adhesive (through a gluing machine) into a drying tunnel, the drying tunnel is 50m long, divided into 4 sections, each section is 12.5m, and the baking temperature range is 75°C to 175°C, wherein: the first section is 75°C to 95°C, the second section is 105°C to 135°C, the third section is 135°C to 175°C, and the fourth section is 85°C to 110°C, and the speed of the gluing machine is 5m / min to 25m / min.
[0033] Another aspect of the present invention is a method for preparing a lightweight melamine insulation board, wherein the ingredients in step a are:
[0034] The melamine resin is a highly etherified melamine formaldehyde resin [the production and providing enterprises and product models (brands) of the highly etherified melamine formaldehyde resin include: JY-303 of Jining Juyue New Materials Co., Ltd., CYMEL303LF of Allnew, etc.;
[0035] The polyether-modified epoxy resin is produced by: Japanese ADEKA's EP-1307, EP-4000, etc.
[0036] The organic silicone resin, the production and providing enterprises and product models (brands) of the organic silicone resin are: SI-101 of Laiyang Shengbang Organic Silicon Technology Co., Ltd., KR-271 of Shin-Etsu Chemical Co., Ltd. of Japan, SM1153D of Sanmu Group, etc.;
[0037] The melamine salt is phosphate [the production and provision of the phosphate include: Jinan Taizhong Kexing New Material Technology Co., Ltd., Guangzhou Shanghe Chemical Technology Co., Ltd.'s X2023, etc.], polyphosphate [the production and provision of the polyphosphate include: Hubei Longxin Chemical Industry Co., Ltd.'s LX9685, Zhongshan Dixin Chemical Co., Ltd.'s DBFPE, etc.], ammonium polyphosphate [the production and provision of the ammonium polyphosphate include: Guangzhou Yinyuan New Materials Co., Ltd. FR-AP1001 of Jinan Xinnuo Chemical Co., Ltd., APP of Jinan Haobang Chemical Co., Ltd., etc.], dimelamine pyrophosphate [the production and product models (brands) of the dimelamine pyrophosphate are: Senfida Chemical, Wuhan Huaxiang Kejie Biotechnology Co., Ltd., etc.], melamine cyanurate [the production and product models (brands) of the melamine cyanurate are: Guangzhou Yinyuan New Materials Co., Ltd., Shandong Qizhuo New Materials Technology Co., Ltd., etc.] any one or a mixture of two or more thereof;
[0038] The curing agent is a mixture of any two or more of diaminodiphenyl sulfone [the production and provision of diaminodiphenyl sulfone include: DDS of Jingmen Dongxin Biotechnology Co., Ltd., PA04296 of Guangdong Wengjiang Biotechnology Co., Ltd., etc.], dicyandiamide [the production and provision of dicyandiamide include: Jinan Kaichuang Chemical Co., Ltd., Guangzhou Xinxi Metallurgical Chemical Co., Ltd., etc.], and diaminodiphenylmethane [the production and provision of diaminodiphenylmethane include: Wuhan Zhisheng Technology Co., Ltd., Zhangjiagang Yarui Chemical Co., Ltd., Guangzhou Yangming Chemical Technology Co., Ltd., etc.];
[0039] The nano-modifier is one or a mixture of two of fumed silica [the fumed silica is produced by companies and product models (brands): TT 1000granulate of Suzhou Unocal Insulation Technology Co., Ltd.] and hollow glass microspheres [the hollow glass microspheres are produced by companies and product models (brands): C-40 of Zhongke Huaxing New Materials Co., Ltd., S4630 of 3M Company, etc.];
[0040] The modifying agent is any one of 3-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-aminopropyl triethoxysilane include: Shandong Tianming Biotechnology Development Co., Ltd., Shandong Xiya Chemical Co., Ltd., Linyi Azeroth Biotechnology Co., Ltd., etc.], 3-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-glycidyloxypropyl trimethoxysilane include: Hubei Yongkuo Technology Co., Ltd., Nantong Runfeng Petrochemical Co., Ltd., Guangdong Wengjiang Chemical Reagent Co., Ltd., etc.], γ-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-aminopropyl triethoxysilane include: Hangzhou Jessica Chemical Co., Ltd., Henan Wanshan New Materials Technology Co., Ltd., etc.], γ-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-glycidyloxypropyl trimethoxysilane include: Henan Xinpeng Chemical Products Co., Ltd., Henan Xiye Chemical Co., Ltd., etc.] or a mixture of two or more thereof;
[0041] The accelerator is any one of imidazole [the production and provision of the imidazole include: 2-methylimidazole of Linyi Mingpin Chemical Co., Ltd., N,N'-carbonyldiimidazole of Shanghai Nuotai Chemical Co., Ltd., etc.], acetyl metal complex [the production and provision of the acetyl metal complex include: No. 3 curing agent of Hubei Hongfuda Biotechnology Co., Ltd., etc.], boron trifluoride ethylamine [the production and provision of boron trifluoride ethylamine include: Beijing Xinao Xunchi Chemical Co., Ltd., Nanjing Chemical Reagent Co., Ltd., etc.], p-toluenesulfonic acid [the production and provision of p-toluenesulfonic acid include: Datang Chemical Co., Ltd., Ji Chuang Chemical Co., Ltd., Shandong Dongyue New Materials Technology Co., Ltd., etc.], methanesulfonic acid [the production and provision of methanesulfonic acid include: Langyu Chemical, Jinan Ronghui Chemical, etc.] or a mixture of two or more thereof;
[0042] The solvent is toluene [the toluene production and providing enterprises and product models (brands) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd., etc.], xylene [the xylene production and providing enterprises and product models (brands) include: Shandong Ruigang Chemical Co., Ltd., Shandong Guanyi Chemical Co., Ltd., etc.], acetone [the acetone production and providing enterprises and product models (brands) include: Jinan Daliang Chemical Co., Ltd., Kunshan Minglong Chemical Co., Ltd.], butanone [the butanone production and providing enterprises and product models (brands) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd. etc.], ethanol [the production and provision of ethanol and the product models (trademarks) include: Foshan Changxing New Materials Co., Ltd., Shandong Xinhongfeng New Materials Technology Co., Ltd., etc.], ethylene glycol methyl ether [the production and provision of ethylene glycol methyl ether and the product models (trademarks) include: Shandong Jinyueyuan New Materials Co., Ltd., Shandong Jinyueyuan New Materials Co., Ltd., etc.], N,N-dimethylformamide [the production and provision of N,N-dimethylformamide and the product models (trademarks) include: Dongguan Nanjian Fine Chemical Co., Ltd., Guangzhou Futuo Trading Co., Ltd., etc.] any one or a mixture of two or more thereof.
[0043] In another aspect of the present invention, the performance parameters of the obtained lightweight melamine insulation board are: bending strength at room temperature is 350MPa-420MPa, bending strength at 150°C is 207MPa-266MPa, tensile strength is 336MPa-372MPa, notched impact strength is 65KJ / m 2 ~75KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m·k, density is 1.52g / cm 3 ~1.75g / cm 3 The thickness of the plate is thin (may be greater than or equal to 0.5 mm).
[0044] In another aspect of the present invention: in the modified melamine thermal insulation resin fiber fabric prepreg described in step c: the weight percentage of the modified melamine thermal insulation resin adhesive is 25% to 50%, and the weight percentage of the basalt fiber fabric is 50% to 75%.
[0045] Compared with the prior art, the present invention has the following characteristics and beneficial effects:
[0046] (1) The lightweight melamine insulation board of the present invention is based on highly etherified melamine formaldehyde resin, silicone resin, and polyether modified epoxy resin, supplemented with modified resin and nano-modifier to improve the overall microscopic topological structure of the system, combined with a high-performance curing agent, and supplemented with high-performance basalt fiber fabric on the basis of simple medium and low temperature modification and grafting, so as to achieve the laminate with excellent halogen-free flame retardancy and insulation, especially high temperature resistance, low thermal conductivity and excellent impact toughness, so as to obtain a lightweight insulation board with excellent comprehensive performance;
[0047] (2) The present invention uses a mixed resin (such as melamine formaldehyde resin, silicone resin, polyether modified epoxy resin) as the matrix and uses ultrafine nano inorganic materials for modification, replacing the usual organic foaming agent foaming to improve thermal insulation, achieving better thermal insulation performance (thermal conductivity at 25°C reaches 0.131w / m·k0.141w / m·k) than common hard insulation boards (usually, thermal conductivity at 25°C is greater than or equal to 0.45w / m·k). At the same time, it also effectively solves the problem of thick thickness of existing common organic or inorganic foamed boards (usually greater than or equal to 8mm), and achieves a thickness range of greater than or equal to 0.5mm for thermal insulation boards, so that they can be more widely used in electronic appliances and industries with high requirements for product intensiveness;
[0048] (3) The present invention makes full use of the combined effect of the dilution effect of the self-released gas and its own heat covering effect when the material is heated and burned, and achieves a highly efficient flame retardant effect (reaching UL94V-0) without adding any flame retardant additives. It breaks through the problem that the existing common foaming materials are easy to burn and have heavy smoke when burning, and meets the urgent requirements of my country for the "green" development of modern industry. At the same time, the present invention also solves the industry consensus that the addition of flame retardant additives significantly reduces the mechanical strength of the material, especially its temperature resistance, and produces a new type of thermal insulation material with excellent comprehensive performance (excellent mechanical strength, which can refer to the bending strength at 23℃±2℃ reaching 350MPa420MPa, and the bending strength at 150℃±2℃ reaching 207MPa266MPa, that is: the bending strength retention rate at 150℃±2℃ is greater than or equal to 57%, and the thermal conductivity at 25℃ reaches 0.131w / m·k0.141w / m·k);
[0049] (4) The present invention uses basalt fiber fabric instead of common glass fiber, which ensures that the board has low thermal conductivity while achieving excellent mechanical strength, especially impact toughness (which can be: impact strength, notched specimen, up to 65KJ / m 2 75KJ / m 2); solves the problem that adding rubber elastomer additives often reduces the overall mechanical strength and heat resistance of the material (for example: Ma Tianxin and Jiang Bo's "The Effect of Toughening Agents on the Performance of Epoxy Resins");
[0050] (5) In the lightweight melamine insulation board of the present invention, during the preparation process of the modified melamine insulation resin adhesive, the raw materials are gradually added by a medium-low temperature synthesis reaction method, and stirred and mixed at medium-low temperature to obtain a uniform modified melamine insulation resin adhesive that meets the prepreg preparation process, and the preparation process is simple;
[0051] (6) The present invention mainly adopts melamine resin, which is modified and then impregnated with basalt fiber fabric to obtain a new type of thermal insulation material with excellent thermal insulation properties, good mechanical strength, insulation and flame retardancy, especially better bending strength, tensile strength and impact toughness. At the same time, it also solves the problem that the thermal insulation material obtained by the existing foaming process is thick and has poor mechanical strength. The lightweight melamine insulation board of the present invention has light weight (density is 1.52g / cm 3 ~1.75g / cm 3 ), high thermal insulation (thermal conductivity (25°C) less than 0.2w / m·k), high strength (flexural strength of 350MPa~420MPa, tensile strength of 336MPa~372MPa), high heat resistance (flexural strength at 150°C 207MPa~266MPa), high toughness (notch impact strength of 65KJ / m 2 ~75KJ / m 2 ), excellent insulation (insulation resistance greater than or equal to 10 8 MΩ), flame retardancy (reaching UL94 V-0 level) and thin sheet thickness (can be greater than or equal to 0.5mm);
[0052] (7) The preparation process of the product of the present invention is simple, and the requirements for production equipment and operators are low. It can better meet my country's requirements for "green, environmentally friendly and efficient" production of enterprises, and greatly reduce production costs and simplify the process. The product quality and performance are excellent, and the actual use value and application prospects are good. The prepared lightweight melamine insulation board is particularly suitable for use as a lightweight insulation material in the fields of new energy vehicles, lithium battery packs, submarine pipeline transportation, etc., and has strong practicality. DETAILED DESCRIPTION
[0053] The following embodiments are intended to further illustrate the present invention, but should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0054] In the following Examples 1-19, the unit of “parts by weight” is “gram”.
[0055] Embodiment 1:
[0056] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0057] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 16 parts by weight of silicone resin, 5 parts by weight of polyether modified epoxy resin, 7 parts by weight of melamine salt (polyphosphate), 13 parts by weight of nano modifier (fumed silica), 0.017 parts by weight of modification agent (γ-aminopropyltriethoxysilane), 1.5 parts by weight of curing agent (diaminodiphenyl sulfone), 0.012 parts by weight of accelerator (imidazole) and 82 parts by weight of solvent (methyl ethyl ketone);
[0058] b. Preparation of modified melamine thermal insulation resin adhesive: at 60°C, nano modifier, modification agent, polyether modified epoxy resin and silicone resin were stirred and mixed at a speed of 850 r / min, stirred for 1.25 hours, and then a curing agent was added and mixed at room temperature, stirred for 0.65 hours, and then melamine resin and melamine salt were added, mixed and stirred at room temperature, stirred for 1 hour, and then a solvent and an accelerator were added, mixed and stirred at room temperature, and the resin molding time was tested at 160°C for 366 seconds to obtain a modified melamine thermal insulation resin adhesive;
[0059] c. Preparing modified melamine thermal insulation resin fiber fabric prepreg: coating the modified melamine thermal insulation resin adhesive prepared in step b on basalt fiber fabric through a glue coating machine, and then placing the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive into a drying tunnel, wherein the drying tunnel is 50 m long and divided into 4 sections, each section is 12.5 m, and the baking temperature range is 75° C. to 175° C., wherein: the first section is 75° C. to 95° C., the second section is 105° C. to 135° C., the third section is 135° C. to 175° C., and the fourth section is 85° C. to 110° C. The speed of the glue coating machine is 5 m / min to 25 m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained; the drying tunnel is pre-baked before baking; the soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0060] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0061] Embodiment 2:
[0062] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0063] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 19 parts by weight of silicone resin, 8 parts by weight of polyether modified epoxy resin, 5 parts by weight of melamine salt (melamine cyanurate), 15 parts by weight of nano modifier (hollow glass microspheres), 0.013 parts by weight of modification agent (3-glycidyloxypropyltrimethoxysilane), 0.2 parts by weight of curing agent (dicyandiamide), 0.032 parts by weight of accelerator (acetyl metal complex) and 91 parts by weight of solvent (N,N-dimethylformamide);
[0064] b. Preparation of modified melamine thermal insulation resin adhesive: at a temperature of 55° C., the nano modifier, the modifying agent, the polyether modified epoxy resin and the silicone resin were stirred and mixed at a speed of 800 r / min, stirred for 1.75 h, and then a curing agent was added and mixed and stirred at room temperature, stirred for 0.5 h, and then melamine resin and melamine salt were added, mixed and stirred at room temperature, stirred for 1.15 h, and then a solvent and an accelerator were added, mixed and stirred at room temperature, and the resin molding time was tested to be 347 s at 160° C. to obtain a modified melamine thermal insulation resin adhesive;
[0065] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0066] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0067] Embodiment 3:
[0068] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0069] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 15 parts by weight of silicone resin, 11 parts by weight of polyether modified epoxy resin, 13 parts by weight of melamine salt (phosphate), 11 parts by weight of nano modifier (hollow glass microspheres), 0.01 parts by weight of modification agent (γ-aminopropyltriethoxysilane), 0.4 parts by weight of curing agent (diaminodiphenylmethane), 0.005 parts by weight of accelerator (boron trifluoride ethylamine) and 60 parts by weight of solvent (toluene);
[0070] b. Preparation of modified melamine thermal insulation resin adhesive: at a temperature of 50° C., the nano modifier, the modifying agent, the polyether modified epoxy resin and the silicone resin were stirred and mixed at a speed of 900 r / min, stirred for 2.5 hours, and then a curing agent was added and mixed and stirred at room temperature, stirred for 0.75 hours, and then melamine resin and melamine salt were added, mixed and stirred at room temperature, stirred for 0.75 hours, and then a solvent and an accelerator were added, mixed and stirred at room temperature, and the resin molding time was tested at 160° C. for 372 seconds to obtain a modified melamine thermal insulation resin adhesive;
[0071] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0072] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0073] Embodiment 4:
[0074] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0075] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 21 parts by weight of silicone resin, 9 parts by weight of polyether modified epoxy resin, 11 parts by weight of melamine salt (ammonium polyphosphate), 10 parts by weight of nano modifier (fumed silica), 0.023 parts by weight of modifying agent (3-aminopropyltriethoxysilane), 0.9 parts by weight of curing agent (diaminodiphenyl sulfone), 0.021 parts by weight of accelerator (p-toluenesulfonic acid) and 125 parts by weight of solvent (ethanol);
[0076] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 65° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1200 r / min, stirred for 1 hour (to prepare the modified resin for standby use), and then a curing agent was added and mixed and stirred at room temperature, and after stirring for 0.75 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature, and after stirring for 1 hour, a solvent and an accelerator were added, and mixed and stirred at room temperature, and the resin molding time was tested at 160° C. for 320 seconds to obtain a modified melamine heat-insulating resin adhesive;
[0077] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0078] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0079] Embodiment 5:
[0080] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0081] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 18 parts by weight of silicone resin, 15 parts by weight of polyether modified epoxy resin, 9 parts by weight of melamine salt (dimelamine pyrophosphate), 19 parts by weight of nano modifier (fumed silica), 0.026 parts by weight of modification agent (3-aminopropyltriethoxysilane), 1.3 parts by weight of curing agent (diaminodiphenyl sulfone), 0.041 parts by weight of accelerator (methanesulfonic acid) and 103 parts by weight of solvent (xylene);
[0082] b. Preparation of modified melamine thermal insulation resin adhesive: at a temperature of 55°C, the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1100 r / min, stirred for 2 hours, and then the curing agent was added and mixed and stirred at room temperature, stirred for 0.5 hours, and then the melamine resin and the melamine salt were added and mixed and stirred at room temperature, stirred for 0.75 hours, and then the solvent and the accelerator were added and mixed and stirred at room temperature, and the resin molding time was tested at 160°C for 338 seconds to obtain a modified melamine thermal insulation resin adhesive;
[0083] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0084] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0085] Embodiment 6:
[0086] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0087] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 17 parts by weight of silicone resin, 18 parts by weight of polyether modified epoxy resin, melamine salt (5 parts by weight of polyphosphate and 5 parts by weight of dimelamine pyrophosphate), 21 parts by weight of nano modifier (hollow glass microspheres), 0.019 parts by weight of modification treatment agent (3-glycidyloxypropyltrimethoxysilane), 2.1 parts by weight of curing agent (dicyandiamide), accelerator (0.011 parts by weight of imidazole and 0.025 parts by weight of boron trifluoride ethylamine) and solvent (116 parts by weight of ethylene glycol methyl ether);
[0088] b. Preparation of modified melamine heat-insulating resin adhesive: at 70° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1150 r / min, and the modified resin was prepared for standby after stirring for 2.5 hours, and then a curing agent was added and mixed and stirred at room temperature, and after stirring for 1 hour, melamine resin and melamine salt were added, and mixed and stirred at room temperature, and after stirring for 1 hour, a solvent and an accelerator were added, and mixed and stirred at room temperature, and the resin molding time was tested to be 351s at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0089] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0090] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0091] Embodiment 7:
[0092] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0093] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 20 parts by weight of silicone resin, 13 parts by weight of polyether modified epoxy resin, melamine salt (2 parts by weight of melamine cyanurate and 6 parts by weight of ammonium polyphosphate), 26 parts by weight of nano modifier (fumed silica), 0.015 parts by weight of modification agent (γ-aminopropyltriethoxysilane), 3.6 parts by weight of curing agent (diaminodiphenylmethane), accelerator (0.021 parts by weight of imidazole and 0.031 parts by weight of acetyl metal complex) and 177 parts by weight of solvent (acetone);
[0094] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 65° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1350 r / min, and the modified resin was prepared for standby after stirring for 2.25 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 1.25 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature. After stirring for 1.2 hours, a solvent and an accelerator were added, and mixed and stirred at room temperature. The resin molding time was tested to be 382 seconds at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0095] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0096] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0097] Embodiment 8:
[0098] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0099] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 28 parts by weight of silicone resin, 20 parts by weight of polyether modified epoxy resin, melamine salt (5 parts by weight of melamine cyanurate and 1 part by weight of polyphosphate), 23 parts by weight of nano modifier (fumed silica), 0.021 parts by weight of modification agent (γ-glycidyloxypropyltrimethoxysilane), curing agent (4.9 parts by weight of diaminodiphenylmethane and 5 parts by weight of dicyandiamide), accelerator (0.007 parts by weight of toluenesulfonic acid and 0.04 parts by weight of imidazole) and solvent (73 parts by weight of acetone and 73 parts by weight of xylene);
[0100] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 75° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1400 r / min, and the modified resin was prepared for standby after stirring for 1.5 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 1.5 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature. After stirring for 1 hour, a solvent and an accelerator were added, and mixed and stirred at room temperature. The resin molding time was tested to be 401s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0101] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0102] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0103] Embodiment 9:
[0104] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0105] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 22 parts by weight of silicone resin, 17 parts by weight of polyether modified epoxy resin, melamine salt (12 parts by weight of polyphosphate and 7 parts by weight of phosphate), 25 parts by weight of nano modifier (hollow glass microspheres), 0.029 parts by weight of modification agent (γ-aminopropyltriethoxysilane), curing agent (2 parts by weight of diaminodiphenyl sulfone and 1.1 parts by weight of diaminodiphenylmethane), accelerator (0.047 parts by weight of imidazole, 0.053 parts by weight of methanesulfonic acid) and solvent (173 parts by weight of toluene and 19 parts by weight of ethanol);
[0106] b. Preparation of modified melamine heat-insulating resin adhesive: at 70° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1250 r / min, and the modified resin was prepared for standby after stirring for 1.45 h. A curing agent was added and mixed at room temperature. After stirring for 1 h, melamine resin and melamine salt were added and mixed at room temperature. After stirring for 1.05 h, a solvent and an accelerator were added and mixed at room temperature. The resin molding time was tested to be 394 s at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0107] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0108] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0109] Embodiment 10:
[0110] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0111] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 25 parts by weight of silicone resin, 21 parts by weight of polyether modified epoxy resin, melamine salt (7 parts by weight of phosphate, 14 parts by weight of ammonium polyphosphate), 28 parts by weight of nano modifier (fumed silica), modifying agent (0.013 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.02 parts by weight of 3-aminopropyltriethoxysilane), curing agent (4 parts by weight of diaminodiphenyl sulfone and 0.4 parts by weight of dicyandiamide), accelerator (0.038 parts by weight of acetyl metal complex and 0.025 parts by weight of boron trifluoride ethylamine) and solvent (166 parts by weight of toluene and 42 parts by weight of N,N-dimethylformamide);
[0112] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 60° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 950 r / min, and the modified resin was prepared for standby after stirring for 2.5 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 1.65 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature. After stirring for 1.25 hours, a solvent and an accelerator were added, and mixed and stirred at room temperature. The resin molding time was tested to be 414 seconds at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0113] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0114] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0115] Embodiment 11:
[0116] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0117] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 23 parts by weight of silicone resin, 25 parts by weight of polyether modified epoxy resin, melamine salt (6 parts by weight of melamine cyanurate and 10 parts by weight of phosphate), nano modifier (11 parts by weight of hollow glass microspheres and 20 parts by weight of fumed silica), modification treatment agent (0.022 parts by weight of γ-glycidyloxypropyltrimethoxysilane and 0.015 parts by weight of 3-aminopropyltriethoxysilane), curing agent (1.9 parts by weight of dicyandiamide and 3 parts by weight of diaminodiphenyl sulfone), accelerator (0.048 parts by weight of acetyl metal complex, 0.021 parts by weight of p-toluenesulfonic acid) and solvent (91 parts by weight of acetone, 90 parts by weight of ethanol and 90 parts by weight of ethylene glycol methyl ether);
[0118] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 75° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1350 r / min, and the modified resin was prepared for standby after stirring for 2.75 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 2 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature. After stirring for 1 hour, a solvent and an accelerator were added, and mixed and stirred at room temperature. The resin molding time was tested to be 406 s at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0119] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0120] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0121] Embodiment 12:
[0122] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0123] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 26 parts by weight of silicone resin, 22 parts by weight of polyether modified epoxy resin, melamine salt (11 parts by weight of melamine cyanurate and 7 parts by weight of dimelamine pyrophosphate), nano modifier (5 parts by weight of hollow glass microspheres and 30 parts by weight of fumed silica), modification agent (0.03 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.013 parts by weight of γ-glycidyloxypropyltrimethoxysilane), curing agent (2.8 parts by weight of diaminodiphenyl sulfone and 2.8 parts by weight of diaminodiphenylmethane), accelerator (0.037 parts by weight of methylsulfonic acid and 0.034 parts by weight of acetyl metal complex) and solvent (98 parts by weight of acetone, 62 parts by weight of xylene and 87 parts by weight of N,N-dimethylformamide);
[0124] b. Preparation of modified melamine heat-insulating resin adhesive: at 80° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1500 r / min, and the modified resin was prepared for standby after stirring for 2.75 h. A curing agent was added and mixed at room temperature. After stirring for 1.75 h, melamine resin and melamine salt were added and mixed at room temperature. After stirring for 1.45 h, a solvent and an accelerator were added and mixed at room temperature. The resin molding time was tested to be 421 s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0125] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0126] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0127] Embodiment 13:
[0128] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0129] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 30 parts by weight of silicone resin, 28 parts by weight of polyether modified epoxy resin, melamine salt (5 parts by weight of ammonium polyphosphate and 12 parts by weight of dimelamine pyrophosphate), nano modifier (12 parts by weight of fumed silica and 20 parts by weight of hollow glass microspheres), modification agent (0.041 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.01 parts by weight of γ-aminopropyltriethoxysilane), curing agent (5.2 parts by weight of diaminodiphenyl sulfone and 2.2 parts by weight of dicyandiamide), accelerator (0.057 parts by weight of p-toluenesulfonic acid and 0.021 parts by weight of boron trifluoride ethylamine) and solvent (71 parts by weight of toluene, 88 parts by weight of butanone, 132 parts by weight of acetone);
[0130] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 65° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1000 r / min, and the modified resin was prepared for standby after stirring for 1.25 h. A curing agent was added and mixed at room temperature. After stirring for 2.15 h, melamine resin and melamine salt were added, and the mixture was mixed and stirred at room temperature. After stirring for 1.05 h, a solvent and an accelerator were added, and the mixture was mixed and stirred at room temperature. The resin molding time was tested to be 411 s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0131] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0132] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0133] Embodiment 14:
[0134] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0135] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 24 parts by weight of silicone resin, 24 parts by weight of polyether modified epoxy resin, melamine salt (11 parts by weight of melamine cyanurate and 13 parts by weight of ammonium polyphosphate), nano modifier (22 parts by weight of hollow glass microspheres and 15 parts by weight of fumed silica), modification treatment agent (0.026 parts by weight of γ-aminopropyltriethoxysilane and 0.022 parts by weight of γ-glycidyloxypropyltrimethoxysilane), curing agent (0.6 parts by weight of diaminodiphenylmethane and 6 parts by weight of dicyandiamide), accelerator (0.028 parts by weight of methylsulfonic acid and 0.064 parts by weight of boron trifluoride ethylamine) and solvent (41 parts by weight of xylene, 127 parts by weight of acetone, 66 parts by weight of ethanol and 72 parts by weight of N,N-dimethylformamide);
[0136] b. Preparation of modified melamine heat-insulating resin adhesive: at 60° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1100 r / min, and the modified resin was prepared for standby after stirring for 2.45 h. Then, a curing agent was added and mixed at room temperature. After stirring for 1.45 h, melamine resin and melamine salt were added, and the mixture was mixed and stirred at room temperature. After stirring for 1 h, a solvent and an accelerator were added, and the mixture was mixed and stirred at room temperature. The resin molding time was tested to be 450 s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0137] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0138] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0139] Embodiment 15:
[0140] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0141] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 27 parts by weight of silicone resin, 26 parts by weight of polyether modified epoxy resin, melamine salt (4.5 parts by weight of melamine cyanurate and 10.5 parts by weight of phosphate), nano modifier (27 parts by weight of fumed silica and 12 parts by weight of hollow glass microspheres), modifying agent (0.01 parts by weight of 3-aminopropyltriethoxysilane, 3 -glycidyloxypropyltrimethoxysilane 0.027 weight parts and γ-glycidyloxypropyltrimethoxysilane 0.015 weight parts), curing agent (diaminodiphenyl sulfone 8.2 weight parts and dicyandiamide 0.9 weight parts), accelerator (methanesulfonic acid 0.05 weight parts, p-toluenesulfonic acid 0.05 weight parts) and solvent (ethylene glycol methyl ether 23 weight parts, ethanol 115 weight parts, butanone 80 weight parts and acetone 109 weight parts);
[0142] b. Preparation of modified melamine heat-insulating resin adhesive: at 85° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1300 r / min, and the modified resin was prepared for standby after stirring for 3 hours, and then a curing agent was added and mixed and stirred at room temperature, and after stirring for 2 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature, and after stirring for 1.25 hours, a solvent and an accelerator were added, and mixed and stirred at room temperature, and the resin molding time was tested to be 389 s at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0143] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0144] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0145] Embodiment 16:
[0146] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0147] a. Ingredients: 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 34 parts by weight of silicone resin, 28 parts by weight of polyether-modified epoxy resin, melamine salt (9 parts by weight of polyphosphate, 3 parts by weight of ammonium polyphosphate and 8 parts by weight of dimelamine pyrophosphate), nano-modifier (26 parts by weight of fumed silica and 7 parts by weight of hollow glass microspheres), modifying agent (0.02 parts by weight of 3-glycidyloxypropyltrimethoxysilane, 0.03 parts by weight of γ-glycidyloxypropyltrimethoxysilane, 0.06 parts by weight of γ-glycidyloxypropyltrimethoxysilane, 0.07 parts by weight of γ-glycidyloxypropyltrimethoxysilane, 0.08 parts by weight of γ-glycidyloxypropyltrimethoxysilane, 0.06 parts by weight of γ-glycidyloxypropyltrimethoxysilane, 0.08 ... 0.02 parts by weight of hydroglyceryl ether oxide propyl trimethoxy silane and 0.02 parts by weight of γ-aminopropyl triethoxy silane), a curing agent (3.6 parts by weight of dicyandiamide and 5.3 parts by weight of diaminodiphenylmethane), an accelerator (0.033 parts by weight of acetyl metal complex, 0.035 parts by weight of imidazole and 0.026 parts by weight of boron trifluoride ethylamine) and a solvent (97 parts by weight of toluene, 91 parts by weight of butanone, 44 parts by weight of ethanol, 65 parts by weight of acetone and 65 parts by weight of xylene);
[0148] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 75° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1400 r / min, and the modified resin was prepared for standby after stirring for 2 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 2.5 hours, melamine resin and melamine salt were added, and the mixture was mixed and stirred at room temperature. After stirring for 1.15 hours, a solvent and an accelerator were added, and the mixture was mixed and stirred at room temperature. The resin molding time was tested to be 396 seconds at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0149] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0150] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0151] Embodiment 17:
[0152] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0153] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 29 parts by weight of silicone resin, 35 parts by weight of polyether modified epoxy resin, melamine salt (5 parts by weight of ammonium polyphosphate, 11 parts by weight of dimelamine pyrophosphate and 9 parts by weight of melamine cyanurate), nano modifier (20 parts by weight of hollow glass microspheres and 20 parts by weight of fumed silica), modification treatment agent (0.005 parts by weight of 3-aminopropyltriethoxysilane, 0.01 parts by weight of 3-glycidyloxypropyltrimethoxysilane) and 0.02 parts by weight of 1.5-hydroxy-2-nitro-1-ol (2-nitro-1-ol)-1-ol (2-nitro-1-ol)-1-ol (2-nitro-1-ol)-1-ol (2-nitro-1-ol)-1-ol 0.017 parts by weight, γ-aminopropyltriethoxysilane 0.034 parts by weight), a curing agent (4.4 parts by weight of diaminodiphenyl sulfone, 3.5 parts by weight of diaminodiphenylmethane and 4.1 parts by weight of dicyandiamide), an accelerator (0.022 parts by weight of acetyl metal complex, 0.051 parts by weight of boron trifluoride ethylamine and 0.016 parts by weight of p-toluenesulfonic acid) and a solvent (57 parts by weight of toluene, 36 parts by weight of butanone, 72 parts by weight of ethylene glycol methyl ether, 117 parts by weight of acetone, 67 parts by weight of N,N-dimethylformamide);
[0154] b. Preparation of modified melamine heat-insulating resin adhesive: at 80° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1200 r / min, stirred for 1.25 h to prepare a modified resin for standby use, and then a curing agent was added and mixed and stirred at room temperature, and after stirring for 2.25 h, melamine resin and melamine salt were added, and mixed and stirred at room temperature, and after stirring for 1.25 h, a solvent and an accelerator were added, and mixed and stirred at room temperature, and the resin molding time was tested to be 417 s at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0155] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0156] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0157] Embodiment 18:
[0158] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0159] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 35 parts by weight of silicone resin, 29 parts by weight of polyether modified epoxy resin, melamine salt (4 parts by weight of polyphosphate, 7 parts by weight of melamine cyanurate, 4 parts by weight of phosphate and 8 parts by weight of ammonium polyphosphate), nano modifier (32 parts by weight of fumed silica and 4 parts by weight of hollow glass microspheres), modification treatment agent (0.016 parts by weight of 3-glycidyloxypropyltrimethoxysilane, 0.016 parts by weight of γ-aminopropyltrimethoxysilane, 0.02 parts by weight of methyl methacrylate), 1.5 parts by weight of methyl methacrylate, ... ethoxysilane 0.014 weight part and γ-glycidyloxypropyltrimethoxysilane 0.024 weight part), curing agent (diaminodiphenyl sulfone 7 weight parts, diaminodiphenylmethane 3 weight parts and dicyandiamide 3 weight parts), accelerator (boron trifluoride ethylamine 0.05 weight part, p-toluenesulfonic acid 0.025 weight part and methanesulfonic acid 0.008 weight part) and solvent (xylene 81 weight parts, butanone 75 weight parts, ethanol 78 weight parts, acetone 81 weight parts and N,N-dimethylformamide 85 weight parts);
[0160] b. Preparation of modified melamine heat-insulating resin adhesive: at 70° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1150 r / min, and the modified resin was prepared for standby after stirring for 1.75 h. A curing agent was added and mixed at room temperature. After stirring for 2 h, melamine resin and melamine salt were added and mixed at room temperature. After stirring for 1.5 h, a solvent and an accelerator were added and mixed at room temperature. The resin molding time was tested to be 436 s at 160° C. to obtain a modified melamine heat-insulating resin adhesive;
[0161] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0162] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0163] Embodiment 19:
[0164] A method for preparing a lightweight melamine insulation board comprises the following steps:
[0165] a. Ingredients: prepare 100 parts by weight of melamine resin (highly etherified melamine formaldehyde resin), 33 parts by weight of silicone resin, 32 parts by weight of polyether modified epoxy resin, melamine salt (3 parts by weight of polyphosphate, 5 parts by weight of melamine cyanurate, 6 parts by weight of phosphate, 4 parts by weight of ammonium polyphosphate and 3 parts by weight of dimelamine pyrophosphate), nano modifier (4 parts by weight of fumed silica and 34 parts by weight of hollow glass microspheres), modifying agent (0.014 parts by weight of γ-aminopropyltriethoxysilane, 0.016 parts by weight of 3-glycidyloxypropyltrimethoxysilane, 0.01 5 parts by weight and γ-glycidyloxypropyltrimethoxysilane 0.015 parts by weight), a curing agent (5 parts by weight of diaminodiphenyl sulfone, 2.5 parts by weight of diaminodiphenylmethane, 4.2 parts by weight of dicyandiamide), an accelerator (0.02 parts by weight of imidazole, 0.021 parts by weight of acetyl metal complex, 0.018 parts by weight of boron trifluoride ethylamine, 0.019 parts by weight of p-toluenesulfonic acid and 0.018 parts by weight of methanesulfonic acid) and a solvent (42 parts by weight of toluene, 34 parts by weight of xylene, 61 parts by weight of butanone, 54 parts by weight of ethanol, 83 parts by weight of acetone, 43 parts by weight of N,N-dimethylformamide and 69 parts by weight of ethylene glycol methyl ether);
[0166] b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 75° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin were stirred and mixed at a speed of 1250 r / min, and the modified resin was prepared for standby after stirring for 2.5 hours, and then a curing agent was added and mixed and stirred at room temperature. After stirring for 2.45 hours, melamine resin and melamine salt were added, and mixed and stirred at room temperature. After stirring for 1.25 hours, a solvent and an accelerator were added, and mixed and stirred at room temperature. The resin molding time was tested to be 334 seconds at 160° C. to prepare a modified melamine heat-insulating resin adhesive;
[0167] c. Preparation of modified melamine thermal insulation resin fiber fabric prepreg: The modified melamine thermal insulation resin adhesive prepared in step b is coated on the basalt fiber fabric through a gluing machine, and then the basalt fiber fabric coated with the modified melamine thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 75℃~175℃, wherein: the first section is 75℃~95℃, the second section is 105℃~135℃, the third section is 135℃~175℃, and the fourth section is 85℃~110℃. The speed of the gluing machine is 5m / min~25m / min, and the modified melamine thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0168] d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight melamine insulation board is obtained.
[0169] The specific process parameters of Examples 1 to 19 and the technical performance test results of the lightweight melamine insulation board are shown in Tables 1, 2 and 3 below respectively:
[0170] Table 1: Example modified melamine thermal insulation resin fiber fabric prepreg preparation process parameters and central control technical indicators
[0171]
[0172]
[0173] Table 2: Lightweight melamine insulation board pressing process parameters
[0174]
[0175] Table 3: Technical performance test data of lightweight melamine insulation boards prepared in Examples 1-19
[0176]
[0177] As shown in Table 1 and Table 2, the lightweight melamine insulation board of the present invention has a bending strength of 350MPa-420MPa at room temperature, a bending strength of 207MPa-266MPa at 150°C, a tensile strength of 336MPa-372MPa, and a notched impact strength of 65KJ / m 2 ~75KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m·k and density is 1.52g / cm 3 ~1.75g / cm 3 , especially suitable for use in the field of lightweight insulation.
[0178] Embodiment 20:
[0179] A lightweight melamine insulation board, which is a lightweight melamine insulation board obtained by hot pressing multiple layers of overlapping modified melamine insulation resin fiber fabric prepreg (the number of layers of the modified melamine insulation resin fiber fabric prepreg is not limited, and can be any one of 1-500 layers as required);
[0180] The modified melamine heat-insulating resin fiber fabric prepreg is obtained by coating the modified melamine heat-insulating resin adhesive on the basalt fiber fabric and then baking;
[0181] The modified melamine heat-insulating resin adhesive is composed of 100 parts by weight of melamine resin, 35 parts by weight of silicone resin, 35 parts by weight of polyether-modified epoxy resin, 25 parts by weight of melamine salt, 40 parts by weight of nano-modifier, 0.06 parts by weight of modification treatment agent, 13 parts by weight of curing agent, 0.1 parts by weight of accelerator and 400 parts by weight of solvent;
[0182] The basalt fiber fabric is any one of basalt fiber plain cloth, basalt fiber twill cloth, basalt fiber gingham cloth, basalt fiber multi-axial cloth and basalt fiber composite cloth.
[0183] Embodiment 21:
[0184] A lightweight melamine insulation board, which is a lightweight melamine insulation board obtained by hot pressing multiple layers of overlapping modified melamine insulation resin fiber fabric prepreg (the number of layers of the modified melamine insulation resin fiber fabric prepreg is not limited, and can be any one of 1-500 layers as required);
[0185] The modified melamine heat-insulating resin fiber fabric prepreg is obtained by coating the modified melamine heat-insulating resin adhesive on the basalt fiber fabric and then baking;
[0186] The modified melamine heat-insulating resin adhesive is composed of 100 parts by weight of melamine resin, 15 parts by weight of silicone resin, 5 parts by weight of polyether-modified epoxy resin, 5 parts by weight of melamine salt, 10 parts by weight of nano-modifier, 0.01 parts by weight of modification treatment agent, 0.2 parts by weight of curing agent, 0.005 parts by weight of accelerator and 60 parts by weight of solvent;
[0187] The basalt fiber fabric is any one of basalt fiber plain cloth, basalt fiber twill cloth, basalt fiber gingham cloth, basalt fiber multi-axial cloth and basalt fiber composite cloth.
[0188] Embodiment 22:
[0189] A lightweight melamine insulation board, which is a lightweight melamine insulation board obtained by hot pressing multiple layers of overlapping modified melamine insulation resin fiber fabric prepreg (the number of layers of the modified melamine insulation resin fiber fabric prepreg is not limited, and can be any one of 1-500 layers as required);
[0190] The modified melamine heat-insulating resin fiber fabric prepreg is obtained by coating the modified melamine heat-insulating resin adhesive on the basalt fiber fabric and then baking;
[0191] The modified melamine heat-insulating resin adhesive is composed of 100 parts by weight of melamine resin, 25 parts by weight of silicone resin, 20 parts by weight of polyether-modified epoxy resin, 15 parts by weight of melamine salt, 25 parts by weight of nano-modifier, 0.035 parts by weight of modification treatment agent, 6.6 parts by weight of curing agent, 0.05 parts by weight of accelerator and 230 parts by weight of solvent;
[0192] The basalt fiber fabric is any one of basalt fiber plain cloth, basalt fiber twill cloth, basalt fiber gingham cloth, basalt fiber multi-axial cloth and basalt fiber composite cloth.
[0193] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
[0194] In the above embodiments: the percentages used, unless otherwise specified, are all weight (mass) percentages or percentages known to those skilled in the art; the proportions used, unless otherwise specified, are all weight (mass) proportions; and the weights may be in grams or kilograms.
[0195] In the above embodiments, the process parameters (temperature, pressure, time, vehicle speed, rotation speed, etc.) and the amount of each component in each step are ranges, and any point can be applied.
[0196] The technical contents not specifically described in the present invention and the above embodiments are the same as the prior art, and the raw materials are all commercially available products.
[0197] The present invention is not limited to the above embodiments, and all of the contents of the present invention can be implemented and have the above good effects.
Claims
1. A lightweight melamine insulation board, characterized in that: The lightweight melamine insulation board is a lightweight melamine insulation board made by hot pressing multiple layers of overlapping modified melamine insulation resin fiber fabric prepreg; The modified melamine heat-insulating resin fiber fabric prepreg is obtained by coating the modified melamine heat-insulating resin adhesive on the basalt fiber fabric and then baking; The modified melamine heat-insulating resin adhesive is composed of 100 parts by weight of melamine resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of polyether-modified epoxy resin, 5-25 parts by weight of melamine salt, 10-40 parts by weight of nano-modifier, 0.01-0.06 parts by weight of modification treatment agent, 0.2-13 parts by weight of curing agent, 0.005-0.1 parts by weight of accelerator and 60-400 parts by weight of solvent; The basalt fiber fabric is at least one of basalt fiber plain cloth, basalt fiber twill cloth, basalt fiber gingham cloth, basalt fiber multi-axial cloth and basalt fiber composite cloth.
2. The lightweight melamine insulation board according to claim 1, characterized in that: In the modified melamine thermal insulation resin adhesive: The melamine resin is a highly etherified melamine formaldehyde resin; The melamine salt is any one of phosphate, polyphosphate, ammonium polyphosphate, dimelamine pyrophosphate, and melamine cyanurate, or a mixture of two or more thereof; The curing agent is any two or more of diaminodiphenyl sulfone, dicyandiamide and diaminodiphenylmethane; The nano modifier is one or a mixture of fumed silica and hollow glass microspheres; The modifying agent is any one of 3-aminopropyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyloxypropyl trimethoxysilane, or a mixture of two or more thereof; The accelerator is any one of imidazole, acetyl metal complex, ethylamine boron trifluoride, p-toluenesulfonic acid, and methanesulfonic acid, or a mixture of two or more thereof; The solvent is any one of toluene, xylene, acetone, butanone, ethanol, ethylene glycol methyl ether, and N,N-dimethylformamide, or a mixture of two or more thereof.
3. The lightweight melamine insulation board according to claim 1 or 2, characterized in that: The hot pressing molding is: after preheating the template at 105°C to 155°C, the modified melamine thermal insulation resin fiber fabric prepreg is overlapped and placed in the template, and after closing the mold, hot pressing molding is performed under the conditions of temperature 130°C to 175°C and pressure 1MPa to 25MPa, and the hot pressing time is 0.5h to 50h.
4. The lightweight melamine insulation board according to claim 1 or 2, characterized in that: The baking method comprises the following steps: placing the basalt fiber fabric coated with the modified melamine heat-insulating resin adhesive into a drying tunnel, wherein the drying tunnel is 50 m long and is divided into 4 sections, each section is 12.5 m long, and the baking temperature ranges from 75° C. to 175° C., wherein the first section is 75° C. to 95° C., the second section is 105° C. to 135° C., the third section is 135° C. to 175° C., and the fourth section is 85° C. to 110° C. The speed of the gluing machine is 5 m / min to 25 m / min.
5. The lightweight melamine insulation board according to claim 1 or 2, characterized in that: The preparation method of the modified melamine thermal insulation resin adhesive is as follows: at a temperature of 50° C. to 85° C., the nano modifier, the modification treatment agent, the polyether modified epoxy resin and the silicone resin are stirred and mixed, after stirring for 1 hour to 3 hours, a curing agent is added and mixed and stirred at room temperature, after stirring for 0.5 hour to 2.5 hours, melamine resin and melamine salt are added, mixed and stirred at room temperature, after stirring for 0.75 hour to 1.5 hour, a solvent and an accelerator are added, and after stirring and mixing at room temperature, the modified melamine thermal insulation resin adhesive is obtained.
6. The lightweight melamine insulation board according to claim 1 or 2, characterized in that: In the modified melamine thermal insulation resin fiber fabric prepreg, the weight percentage of the modified melamine thermal insulation resin adhesive is 25% to 50%, and the weight percentage of the basalt fiber fabric is 50% to 75%.
7. A method for preparing a lightweight melamine insulation board, characterized in that The following steps are involved: a. Ingredients: prepare the raw materials of each component according to the ratio of 100 parts by weight of melamine resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of polyether modified epoxy resin, 5-25 parts by weight of melamine salt, 10-40 parts by weight of nano modifier, 0.01-0.06 parts by weight of modification treatment agent, 0.2-13 parts by weight of curing agent, 0.005-0.1 parts by weight of accelerator and 60-400 parts by weight of solvent; b. Preparation of modified melamine heat-insulating resin adhesive: at a temperature of 50° C. to 85° C., the nano-modifier, the modifying agent, the polyether-modified epoxy resin and the silicone resin are stirred and mixed, stirred for 1 h to 3 h, and then a curing agent is added and mixed and stirred at room temperature, stirred for 0.5 h to 2.5 h, and then melamine resin and melamine salt are added and mixed and stirred at room temperature, stirred for 0.75 h to 1.5 h, and then a solvent and an accelerator are added, and stirred and mixed at room temperature to obtain a modified melamine heat-insulating resin adhesive; c. Preparing a modified melamine thermal insulation resin fiber fabric prepreg: coating the modified melamine thermal insulation resin adhesive prepared in step b on the basalt fiber fabric, and then baking to obtain a modified melamine thermal insulation resin fiber fabric prepreg; The basalt fiber fabric is at least one of basalt fiber plain fabric, basalt fiber twill fabric, basalt fiber woven fabric, basalt fiber multi-axial fabric, and basalt fiber composite fabric; d. Preparation of lightweight melamine insulation board: preheat the template at 105°C to 155°C, overlap the modified melamine insulation resin fiber fabric prepreg and place it in the template, close the mold and perform hot pressing at a temperature of 130°C to 175°C and a pressure of 1MPa to 25MPa for 0.5h to 50h to obtain a lightweight melamine insulation board.
8. The method for preparing the lightweight melamine insulation board according to claim 7, characterized in that: In another aspect of the present invention: the baking is to put the basalt fiber fabric coated with modified melamine insulation resin adhesive into a drying tunnel, the drying tunnel is 50m long, divided into 4 sections, each section is 12.5m, the baking temperature range is 75°C to 175°C, wherein: the first section is 75°C to 95°C, the second section is 105°C to 135°C, the third section is 135°C to 175°C, and the fourth section is 85°C to 110°C, and the speed of the gluing machine is 5m / min to 25m / min.
9. The method for preparing the lightweight melamine insulation board according to claim 7 or 8, characterized in that: Ingredients in step a: The melamine resin is a highly etherified melamine formaldehyde resin; The melamine salt is any one of phosphate, polyphosphate, ammonium polyphosphate, dimelamine pyrophosphate, and melamine cyanurate, or a mixture of two or more thereof; The curing agent is any two or more of diaminodiphenyl sulfone, dicyandiamide and diaminodiphenylmethane; The nano modifier is one or a mixture of fumed silica and hollow glass microspheres; The modifying agent is any one of 3-aminopropyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyloxypropyl trimethoxysilane, or a mixture of two or more thereof; The accelerator is any one of imidazole, acetyl metal complex, ethylamine boron trifluoride, p-toluenesulfonic acid, and methanesulfonic acid, or a mixture of two or more thereof; The solvent is any one of toluene, xylene, acetone, butanone, ethanol, ethylene glycol methyl ether, and N,N-dimethylformamide, or a mixture of two or more thereof.
10. The method for preparing the lightweight melamine insulation board according to claim 7 or 8, characterized in that: In another aspect of the present invention: the performance parameters of the lightweight melamine insulation board are: the bending strength at room temperature is 350MPa ~ 420MPa, flexural strength at 150°C 207MPa ~ 266MPa, tensile strength 336MPa~372MPa, notched impact strength 65KJ / m 2 ~ 75KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m•k, density is 1.52g / cm 3 ~1.75g / cm 3 .
Citation Information
Patent Citations
Preparation method of melamine-modified epoxy resin glass cloth laminated board
CN111572129A
High-toughness wear-resistant light laminated board and preparation method thereof
CN117659618A
Deposited fiber structure and method for producing the same
JP2003268673A
Fire-resistant filler sheet laminates
US4371579A
Melamine resin prepregs and melamine resin laminates based on modified melamine resins
US5206066A
Cited By
Sintering-free rigid heat insulation plate and preparation method thereof
CN122187467A