Lightweight polyimide thermal insulation board and preparation method thereof
Through the hot pressing forming technology of modified polyimide thermally insulating resin fiber fabric, high-strength, low thermal conductivity and excellent insulating flame retardant thermal insulation panels with moderate density were prepared, which solved the thermal runaway of lithium batteries and new energy vehicles. The lack of demand for thermal insulation materials has achieved efficient thermal insulation and safety improvement.
Patent Information
- Application Number
- CN202410978241.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing lithium battery insulation materials are difficult to prevent explosions within 5 minutes when thermally out of control, and cannot meet the needs of new energy vehicles and lithium battery markets for lightweight, high energy density, low thermal conductivity, flame retardancy and high strength. .
Lightweight polyimide heat insulation panels are prepared by hot pressing using multi-layer overlapping modified polyimide heat insulation resin fiber fabrics, using polyimide resin, silicone resin and nanomodifier materials, combined with Aramid fiber fabric forms a heat-insulating plate with excellent insulation and flame retardant properties.
The density is 1.55g/cm3 to 1.75g/cm3, the thermal conductivity is less than 0.2w/m·k, the bending strength is 380MPa to 450MPa, the tensile strength is 365MPa to 387MPa, the notch impact strength is 60KJ/m2 to 70KJ/m2, and the insulation is achieved. Insulated plates with resistance greater than 108MΩ and UL94 V-0 are suitable for new energy vehicles and lithium battery applications.
Smart Images

Figure BDA0004955226630000231 
Figure BDA0004955226630000241 
Figure BDA0004955226630000242
Abstract
Description
Technical Field
[0001] The present invention belongs to laminated boards and their preparation, and relates to a lightweight polyimide thermal insulation board and its preparation method. The lightweight polyimide thermal insulation board of the present invention (prepared) is suitable for use in the fields of transportation, building insulation, energy industry, etc., and is particularly suitable for use as a lightweight thermal insulation material in the fields of new energy vehicles, lithium battery packs, submarine pipeline transportation, etc. Background Art
[0002] Thermal insulation material is a material or a composite of materials with insulating properties and shielding effect on heat flow. It is usually light, loose, porous, and has low thermal conductivity. It is widely used in industry to prevent heat loss in thermal equipment and pipelines, or used under freezing and low temperature conditions, so it is also called thermal insulation or cold insulation material. At the same time, due to its porous or fibrous structure with good sound absorption function, it is also widely used in the construction industry. Lightweight thermal insulation material is a new type of lightweight, efficient, energy-saving and environmentally friendly material. The widespread application of lightweight thermal insulation material will help reduce energy consumption, reduce environmental pollution, and improve economic and social benefits. It is widely used in transportation, building insulation, energy industry and other fields.
[0003] Thermal runaway is the main cause of power battery pack safety accidents. Under high energy density, battery fire or explosion may occur due to battery batch consistency, thermal stability of the material itself, compatibility between battery components, and high flammability of the electrolyte. After a battery cell experiences thermal runaway, the battery system is required to be free of fire and explosion within 5 minutes. To achieve a "5-minute safe escape time", it is necessary to make more improvements to the thermal insulation materials of the battery pack to delay the explosion time of the faulty battery pack. As China's new energy vehicle market and energy storage lithium battery market continue to grow rapidly, the market demand for lithium battery thermal management flame-retardant insulation materials will show a blowout development trend.
[0004] In order to keep up with the trend of increasingly compact volume and weight of battery packs, lithium battery manufacturers have also put forward revolutionary requirements for the battery pack outer packaging separators they use when designing battery packs, requiring continuous optimization of the volume energy density of battery packs, requiring them to ensure that the battery packs are lightweight (low density), have high energy utilization (low thermal conductivity), and have high safety (flame retardant), and in particular, have excellent support strength, deformation resistance (mechanical strength), insulation performance (electrical strength), and thinner sheet thickness (can be greater than or equal to 0.5mm). These are unattainable by foam materials with low mechanical strength and large thickness obtained by existing technologies. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a lightweight polyimide insulation board and a preparation method thereof.3 ~1.75g / cm 3 ), high thermal insulation (thermal conductivity (25°C) less than 0.2w / m·k), high strength (flexural strength of 380MPa~450MPa, tensile strength of 365MPa~387MPa), high heat resistance (flexural strength at 180°C 267MPa~331MPa), high toughness (notch impact strength of 60KJ / m 2 ~70KJ / m 2 ), excellent insulation (insulation resistance greater than or equal to 10 8 The invention discloses a lightweight polyimide heat insulation board with high thermal conductivity, low carbonization temperature and low quenching resistance (MΩ), flame retardancy (reaching UL94 V-0 level) and thin board thickness (which can be greater than or equal to 0.5 mm) and a preparation method thereof.
[0006] The present invention is a lightweight polyimide heat insulation board, which is characterized in that the lightweight polyimide heat insulation board is a lightweight polyimide heat insulation board made by hot pressing multiple layers of overlapping modified polyimide heat insulation resin fiber fabric prepreg (the number of layers of the modified polyimide heat insulation resin fiber fabric prepreg is not limited, and can be 1-500 layers as required);
[0007] The modified polyimide thermal insulation resin fiber fabric prepreg is obtained by coating the modified polyimide thermal insulation resin adhesive on the aramid fiber fabric and then baking;
[0008] The modified polyimide heat-insulating resin adhesive is composed of 100 parts by weight of polyimide resin, 15 to 35 parts by weight of silicone resin, 5 to 35 parts by weight of nano-modifier, 0.04 to 0.13 parts by weight of modification treatment agent, 0.005 to 0.1 parts by weight of accelerator and 50 to 200 parts by weight of solvent;
[0009] The aramid fiber fabric is at least one of aramid fiber plain fabric, aramid fiber twill fabric, aramid fiber gingham fabric, aramid fiber multi-axial fabric, and aramid fiber composite fabric (the production and providing enterprises and product models (brands) of the aramid fiber fabric include: AK-200P, AK-240P of Hephaestus Protection Technology (Guangdong) Co., Ltd., Kevlar fabric of Guangdong Tewilong New Materials Application Co., Ltd., etc.).
[0010] In the modified polyimide thermal insulation resin adhesive in the content of the present invention:
[0011] The polyimide resin is polyimide resin powder [the polyimide resin powder is produced by companies and product models (brands) including: PIPower-I of Lilo Group, PI powder of Wuhan Zhisheng Technology Co., Ltd., etc.];
[0012] The organic silicone resin [the production and supply enterprises and product models (brands) of the organic silicone resin include: SI-101 of Laiyang Shengbang Organic Silicon Technology Co., Ltd., KR-271 of Shin-Etsu Chemical Co., Ltd. of Japan, SM1153D of Sanmu Group, etc.];
[0013] The nano-modifier is one or a mixture of two of fumed silica [the fumed silica is produced by companies and product models (brands): TT 1000granulate of Suzhou Unocal Insulation Technology Co., Ltd.] and hollow glass microspheres [the hollow glass microspheres are produced by companies and product models (brands): C-40 of Zhongke Huaxing New Materials Co., Ltd., S4630 of 3M Company, etc.];
[0014] The modifying agent is any one of 3-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-aminopropyl triethoxysilane include: Shandong Tianming Biotechnology Development Co., Ltd., Shandong Xiya Chemical Co., Ltd., Linyi Azeroth Biotechnology Co., Ltd., etc.], 3-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-glycidyloxypropyl trimethoxysilane include: Hubei Yongkuo Technology Co., Ltd., Nantong Runfeng Petrochemical Co., Ltd., Guangdong Wengjiang Chemical Reagent Co., Ltd., etc.], γ-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-aminopropyl triethoxysilane include: Hangzhou Jessica Chemical Co., Ltd., Henan Wanshan New Materials Technology Co., Ltd., etc.], γ-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-glycidyloxypropyl trimethoxysilane include: Henan Xinpeng Chemical Products Co., Ltd., Henan Xiye Chemical Co., Ltd., etc.] or a mixture of two or more thereof;
[0015] The accelerator is any one of imidazole [the production and provision of the imidazole include: 2-methylimidazole of Linyi Mingpin Chemical Co., Ltd., N,N'-carbonyldiimidazole of Shanghai Nuotai Chemical Co., Ltd., etc.], diaminodiphenylmethane [the production and provision of the diaminodiphenylmethane include: Wuhan Zhisheng Technology Co., Ltd., Zhangjiagang Yarui Chemical Co., Ltd., Guangzhou Yangming Chemical Technology Co., Ltd., etc.], and boron trifluoride ethylamine [the production and provision of the boron trifluoride ethylamine include: Beijing Xinao Xunchi Chemical Co., Ltd., Nanjing Chemical Reagent Co., Ltd., etc.] or a mixture of two or more thereof;
[0016] The solvent is any two of acetone [the acetone production and providing enterprises and product models (trademarks) include: Jinan Daliang Chemical Co., Ltd., Kunshan Minglong Chemical Co., Ltd.], butanone [the butanone production and providing enterprises and product models (trademarks) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd., etc.], N,N-dimethylformamide [the N,N-dimethylformamide production and providing enterprises and product models (trademarks) include: Dongguan Nanjian Fine Chemical Co., Ltd., Guangzhou Futuo Trading Co., Ltd., etc.] and a mixture of two or more thereof.
[0017] In the content of the present invention: the hot pressing molding is: after preheating the template at 145°C to 175°C, the modified polyimide insulation resin fiber fabric prepreg is overlapped (including matching and laminating) and placed in the template, and after the mold is closed, it is hot pressed at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa, and the hot pressing time is 0.5h to 50h (h means hours, the same below).
[0018] In the content of the present invention: the baking is: putting the aramid fiber fabric coated with modified polyimide thermal insulation resin adhesive (through a gluing machine) into a drying tunnel, the drying tunnel is 50m long, divided into 4 sections, each section is 12.5m, the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, the fourth section is 100℃~110℃, and the speed of the gluing machine is 10m / min~25m / min.
[0019] In the content of the present invention: the preparation method of the modified polyimide thermal insulation resin adhesive is: at a temperature of 50°C to 85°C, the nano modifier, the modification treatment agent, the polyimide resin and the silicone resin are stirred and mixed at a speed of 800r / min to 1500r / min, and the modified resin is prepared after stirring for 3h to 5h for standby use. After cooling to room temperature, the solvent and the accelerator are added and stirred and mixed. The resin molding time is tested at 180°C for 150s to 300s (s means seconds, the same below), and the modified polyimide thermal insulation resin adhesive is obtained.
[0020] In the content of the present invention: in the modified polyimide thermal insulation resin fiber fabric prepreg: the weight percentage of the (semi-cured) modified polyimide thermal insulation resin adhesive is 30% to 50%, and the weight percentage of the aramid fiber fabric is 50% to 70%.
[0021] In the context of the present invention: the lightweight polyimide insulation board has a light weight (density of 1.55g / cm 3 ~1.75g / cm 3), high thermal insulation (thermal conductivity (25°C) less than 0.2w / m·k), high strength (flexural strength of 380MPa~450MPa, tensile strength of 365MPa~387MPa), high heat resistance (flexural strength at 180°C 267MPa~331MPa), high toughness (notch impact strength of 60KJ / m 2 ~70KJ / m 2 ), excellent insulation (insulation resistance greater than or equal to 10 8 The invention discloses a lightweight polyimide heat insulation board having the characteristics of high thermal conductivity, low noise, low cost, low cost and low cost, high thermal conductivity ...
[0022] Another aspect of the present invention is: a method for preparing a lightweight polyimide insulation board, which is characterized by comprising the following steps:
[0023] a. Ingredients: prepare the raw materials of each component according to the ratio of 100 parts by weight of polyimide resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of nano modifier, 0.04-0.13 parts by weight of modification treatment agent, 0.005-0.1 parts by weight of accelerator and 50-200 parts by weight of solvent;
[0024] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 50°C to 85°C, the nano-modifier, the modifying agent, the polyimide resin and the silicone resin are stirred and mixed at a speed of 800r / min to 1500r / min, and the modified resin is prepared after stirring for 3h to 5h for standby use. After cooling to room temperature, the solvent and the accelerator are added and stirred and mixed. The resin molding time is tested to be 150s to 300s at 180°C, and the modified polyimide thermal insulation resin adhesive is obtained;
[0025] c. Preparing a modified polyimide thermal insulation resin fiber fabric prepreg: coating the modified polyimide thermal insulation resin adhesive prepared in step b on the aramid fiber fabric, and then baking to obtain the modified polyimide thermal insulation resin fiber fabric prepreg;
[0026] The aramid fiber fabric is at least one of aramid fiber plain fabric, aramid fiber twill fabric, aramid fiber gingham fabric, aramid fiber multiaxial fabric, and aramid fiber composite fabric;
[0027] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, close the mold and perform hot pressing at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa for 0.5h to 50h to obtain a lightweight polyimide insulation board.
[0028] In another aspect of the present invention: the baking is to put the aramid fiber fabric coated with modified polyimide insulation resin adhesive (through a gluing machine) into a drying tunnel, the drying tunnel is 50m long, divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃, and the speed of the gluing machine is 10m / min~25m / min.
[0029] Another aspect of the present invention is a method for preparing a lightweight polyimide heat insulation board, wherein the ingredients in step a are:
[0030] The polyimide resin is polyimide resin powder [the polyimide resin powder is produced by companies and product models (brands) including: PIPower-I of Lilo Group, PI powder of Wuhan Zhisheng Technology Co., Ltd., etc.];
[0031] The organic silicone resin [the production and supply enterprises and product models (brands) of the organic silicone resin include: SI-101 of Laiyang Shengbang Organic Silicon Technology Co., Ltd., KR-271 of Shin-Etsu Chemical Co., Ltd. of Japan, SM1153D of Sanmu Group, etc.];
[0032] The nano-modifier is one or a mixture of two of fumed silica [the fumed silica is produced by companies and product models (brands): TT 1000granulate of Suzhou Unocal Insulation Technology Co., Ltd.] and hollow glass microspheres [the hollow glass microspheres are produced by companies and product models (brands): C-40 of Zhongke Huaxing New Materials Co., Ltd., S4630 of 3M Company, etc.];
[0033] The modifying agent is any one of 3-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-aminopropyl triethoxysilane include: Shandong Tianming Biotechnology Development Co., Ltd., Shandong Xiya Chemical Co., Ltd., Linyi Azeroth Biotechnology Co., Ltd., etc.], 3-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the 3-glycidyloxypropyl trimethoxysilane include: Hubei Yongkuo Technology Co., Ltd., Nantong Runfeng Petrochemical Co., Ltd., Guangdong Wengjiang Chemical Reagent Co., Ltd., etc.], γ-aminopropyl triethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-aminopropyl triethoxysilane include: Hangzhou Jessica Chemical Co., Ltd., Henan Wanshan New Materials Technology Co., Ltd., etc.], γ-glycidyloxypropyl trimethoxysilane [the production and providing enterprises and product models (trademarks) of the γ-glycidyloxypropyl trimethoxysilane include: Henan Xinpeng Chemical Products Co., Ltd., Henan Xiye Chemical Co., Ltd., etc.] or a mixture of two or more thereof;
[0034] The accelerator is any one of imidazole [the production and provision of the imidazole include: 2-methylimidazole of Linyi Mingpin Chemical Co., Ltd., N,N'-carbonyldiimidazole of Shanghai Nuotai Chemical Co., Ltd., etc.], diaminodiphenylmethane [the production and provision of the diaminodiphenylmethane include: Wuhan Zhisheng Technology Co., Ltd., Zhangjiagang Yarui Chemical Co., Ltd., Guangzhou Yangming Chemical Technology Co., Ltd., etc.], and boron trifluoride ethylamine [the production and provision of the boron trifluoride ethylamine include: Beijing Xinao Xunchi Chemical Co., Ltd., Nanjing Chemical Reagent Co., Ltd., etc.] or a mixture of two or more thereof;
[0035] The solvent is any two or a mixture of two or more of acetone [the acetone production and providing enterprises and product models (trademarks) include: Jinan Daliang Chemical Co., Ltd., Kunshan Minglong Chemical Co., Ltd.], butanone [the butanone production and providing enterprises and product models (trademarks) include: Langfang Jinhai Chemical Co., Ltd., Shandong Qixing Chemical Co., Ltd., etc.], and N,N-dimethylformamide [the N,N-dimethylformamide production and providing enterprises and product models (trademarks) include: Dongguan Nanjian Fine Chemical Co., Ltd., Guangzhou Futuo Trading Co., Ltd., etc.].
[0036] In another aspect of the present invention: the performance parameters of the obtained lightweight polyimide insulation board are: bending strength of 380MPa-450MPa at room temperature, bending strength of 267MPa-331MPa at 180°C, tensile strength of 365MPa-387MPa, notched impact strength of 60KJ / m 2 ~70KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m·k, density is 1.55g / cm 3 ~1.75g / cm 3 The thickness of the plate is thin (may be greater than or equal to 0.5 mm).
[0037] In another aspect of the present invention: in the modified polyimide thermal insulation resin fiber fabric prepreg described in step c: the weight percentage of the modified polyimide thermal insulation resin adhesive is 30% to 50%, and the weight percentage of the aramid fiber fabric is 50% to 70%.
[0038] Compared with the prior art, the present invention has the following characteristics and beneficial effects:
[0039] (1) The lightweight polyimide thermal insulation board of the present invention uses polyimide resin and silicone resin as the matrix, supplemented with modified resin and nano-modifier to improve the overall microscopic topological structure of the system, and supplemented with high-performance aramid fiber fabric on the basis of simple medium and low temperature modification and grafting, so as to achieve the laminated board having both excellent halogen-free flame retardancy and insulation, especially high temperature resistance, low thermal conductivity and excellent impact toughness, so as to obtain a thermal insulation lightweight board with excellent comprehensive performance;
[0040] (2) The present invention uses a mixed resin (such as polyimide resin, silicone resin) as the matrix, and uses ultra-fine nano-inorganic materials with a smaller mass ratio (can be: greater than or equal to 3.7% of the total mass of the matrix resin) for modification, replacing the usual organic foaming agent foaming to improve thermal insulation, and achieves better thermal insulation performance (thermal conductivity at 25°C reaches 0.122w / m·k0.136w / m·k) than common hard insulation boards (usually, thermal conductivity at 25°C is greater than or equal to 0.45w / m·k). At the same time, it also effectively solves the problem of thick thickness of existing common organic or inorganic foamed boards (usually greater than or equal to 8mm), and achieves a thickness range of greater than or equal to 0.5mm for thermal insulation boards, so that they can be more widely used in electronic appliances and industries with high requirements for product intensiveness;
[0041] (3) The present invention makes full use of the combined effect of the dilution effect of the self-released gas and its own heat covering effect when the material is heated and burned, and achieves a highly efficient flame retardant effect (reaching UL94V-0) without adding any flame retardant additives. It breaks through the problem that the existing common foaming materials are easy to burn and have heavy smoke when burning, and meets the urgent requirements of my country for the "green" development of modern industry. At the same time, the present invention also solves the industry consensus that the addition of flame retardant additives significantly reduces the mechanical strength of the material, especially its temperature resistance, and produces a new type of thermal insulation material with excellent comprehensive performance (excellent mechanical strength, which can refer to the bending strength at 23℃±2℃ reaching 380MPa450MPa, and the bending strength at 180℃±2℃ reaching 267MPa331MPa, that is: the bending strength retention rate at 180℃±2℃ is greater than or equal to 70%, and the thermal conductivity at 25℃ reaches 0.122w / m·k0.136w / m·k);
[0042] (4) The present invention uses aramid fiber fabric instead of common glass fiber, which ensures that the board has low thermal conductivity and at the same time enables the board to achieve excellent mechanical strength, especially impact toughness (which can be: impact strength, notched specimen, up to 60KJ / m 2 70KJ / m 2). It solves the problem that adding rubber elastomer additives often reduces the overall mechanical strength and heat resistance of the material (for example: Ma Tianxin and Jiang Bo's "The Effect of Toughening Agents on the Performance of Epoxy Resins");
[0043] (5) In the preparation process of the modified polyimide thermal insulation resin adhesive of the lightweight polyimide thermal insulation board of the present invention, the raw materials are gradually added by a medium-low temperature synthesis reaction method, and stirred and mixed at medium-low temperature to obtain a uniform modified polyimide thermal insulation resin adhesive that meets the prepreg preparation process; and the preparation process is simple, and the requirements for production equipment and operators are low, which can better meet my country's requirements for enterprises to produce "green, environmentally friendly, and efficient", and greatly reduce production costs, simplify processes, and have good quality. It has significant practical use value and application prospects;
[0044] (6) The present invention adopts a composite resin (polyimide resin combined with silicone resin) as the main resin, and then impregnates the aramid fiber fabric after modification, thereby obtaining a fabric having better thermal insulation (the thermal conductivity coefficient at 25°C can be 0.122w / m·k0.136w / m·k), good mechanical strength, insulation and flame retardancy, and especially better impact toughness (the impact strength under the notch can be 60KJ / m 2 ~70KJ / m 2 ), low density (density can be 1.55g / cm 3 ~1.75g / cm 3 ) characteristics; at the same time, the present invention also solves the problem of adding less inorganic modifier (specifically, the inorganic modifier may account for 3.7% or more of the total amount of the matrix resin), avoiding the problem that, on the one hand, the mechanical strength of the board is poor (especially in terms of toughness), and on the other hand, it is difficult to mix and stir the resin raw materials and the resin glue is difficult to evenly infiltrate the fibers, which ultimately affects the quality stability of the board;
[0045] (7) The product of the present invention has a simple preparation process, simple procedures, easy operation and strong practicability. DETAILED DESCRIPTION
[0046] The following embodiments are intended to further illustrate the present invention, but should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0047] In the following Examples 1-19, the specific unit of "parts by weight" is "gram".
[0048] Embodiment 1:
[0049] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0050] a. Ingredients: prepare 100 parts by weight of polyimide resin, 17 parts by weight of silicone resin, 7 parts by weight of nano-modifier (hollow glass microspheres), 0.052 parts by weight of modification agent (3-glycidyloxypropyltrimethoxysilane), 0.008 parts by weight of accelerator (imidazole) and solvent (40 parts by weight of N,N-dimethylformamide and 27 parts by weight of butanone);
[0051] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 75° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 950 r / min, and the modified resin was prepared after stirring for 3.25 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 282 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0052] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0053] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0054] Embodiment 2:
[0055] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0056] a. Ingredients: prepare 100 parts by weight of polyimide resin, 18 parts by weight of silicone resin, 5 parts by weight of nano-modifier (fumed silica), 0.07 parts by weight of modifying agent (3-aminopropyltriethoxysilane), 0.005 parts by weight of accelerator (diaminodiphenylmethane) and solvent (39 parts by weight of N,N-dimethylformamide, 39 parts by weight of butanone);
[0057] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 65° C., the nano-modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 800 r / min, and the modified resin was prepared after stirring for 3.15 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 265 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0058] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0059] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0060] Embodiment 3:
[0061] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0062] a. Ingredients: prepare 100 parts by weight of polyimide resin, 16 parts by weight of silicone resin, 11 parts by weight of nano-modifier (fumed silica), 0.04 parts by weight of modifying agent (γ-aminopropyltriethoxysilane), 0.012 parts by weight of accelerator (boron trifluoride ethylamine) and solvent (20 parts by weight of acetone, 30 parts by weight of butanone);
[0063] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 60° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 900 r / min, and the modified resin was prepared after stirring for 3 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 249 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0064] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0065] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0066] Embodiment 4:
[0067] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0068] a. Ingredients: prepare 100 parts by weight of polyimide resin, 15 parts by weight of silicone resin, 9 parts by weight of nano-modifier (hollow glass microspheres), 0.06 parts by weight of modification agent (γ-glycidyloxypropyltrimethoxysilane), 0.015 parts by weight of accelerator (boron trifluoride ethylamine) and solvent (25 parts by weight of butanone, 64 parts by weight of N,N-dimethylformamide);
[0069] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 50° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 850 r / min, and the modified resin was prepared after stirring for 3.25 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 216 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0070] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0071] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0072] Embodiment 5:
[0073] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0074] a. Ingredients: prepare 100 parts by weight of polyimide resin, 22 parts by weight of silicone resin, 15 parts by weight of nano modifier (fumed silica), modifying agent (0.052 parts by weight of 3-aminopropyltriethoxysilane and 0.041 parts by weight of 3-glycidyloxypropyltrimethoxysilane), 0.019 parts by weight of accelerator (imidazole) and solvent (33 parts by weight of acetone, 60 parts by weight of N,N-dimethylformamide);
[0075] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 70° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1050 r / min, and the modified resin was prepared after stirring for 3.65 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 273 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0076] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0077] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0078] Embodiment 6:
[0079] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0080] a. Ingredients: prepare 100 parts by weight of polyimide resin, 21 parts by weight of silicone resin, 12 parts by weight of nano-modifier (hollow glass microspheres), modification treatment agent (0.023 parts by weight of γ-aminopropyltriethoxysilane and 0.05 parts by weight of 3-aminopropyltriethoxysilane), 0.021 parts by weight of accelerator (imidazole) and solvent (10 parts by weight of N,N-dimethylformamide and 92 parts by weight of acetone);
[0081] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 55° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1150 r / min, and the modified resin was prepared after stirring for 4.15 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 258 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0082] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0083] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0084] Embodiment 7:
[0085] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0086] a. Ingredients: prepare 100 parts by weight of polyimide resin, 19 parts by weight of silicone resin, 17 parts by weight of nano modifier (fumed silica), modifying agent (0.035 parts by weight of γ-glycidyloxypropyltrimethoxysilane and 0.041 parts by weight of 3-aminopropyltriethoxysilane), 0.029 parts by weight of accelerator (diaminodiphenylmethane) and solvent (77 parts by weight of acetone and 32 parts by weight of N,N-dimethylformamide);
[0087] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 72° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1000 r / min, and the modified resin was prepared after stirring for 4 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 262 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0088] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0089] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0090] Embodiment 8:
[0091] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0092] a. Ingredients: prepare 100 parts by weight of polyimide resin, 26 parts by weight of silicone resin, 16 parts by weight of nano modifier (fumed silica), modifying agent (0.012 parts by weight of γ-glycidyloxypropyltrimethoxysilane and 0.1 parts by weight of 3-glycidyloxypropyltrimethoxysilane), 0.026 parts by weight of accelerator (diaminodiphenylmethane) and solvent (74 parts by weight of acetone and 42 parts by weight of butanone);
[0093] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 65° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1150 r / min, and the modified resin was prepared after stirring for 4.25 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 209 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0094] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0095] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0096] Embodiment 9:
[0097] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0098] a. Ingredients: prepare 100 parts by weight of polyimide resin, 23 parts by weight of silicone resin, 19 parts by weight of nano-modifier (hollow glass microspheres), modification treatment agent (0.033 parts by weight of γ-aminopropyltriethoxysilane and 0.05 parts by weight of 3-glycidyloxypropyltrimethoxysilane), 0.035 parts by weight of accelerator (boron trifluoride ethylamine) and solvent (81 parts by weight of N,N-dimethylformamide, 38 parts by weight of butanone);
[0099] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 58° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1200 r / min, and the modified resin was prepared after stirring for 3.5 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 184 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0100] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0101] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0102] Embodiment 10:
[0103] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0104] a. Ingredients: prepare 100 parts by weight of polyimide resin, 28 parts by weight of silicone resin, nano modifier (8 parts by weight of fumed silica and 10 parts by weight of hollow glass microspheres), modifying agent (0.009 parts by weight of γ-aminopropyltriethoxysilane and 0.082 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.016 parts by weight of imidazole and 0.016 parts by weight of boron trifluoride ethylamine) and solvent (86 parts by weight of acetone and 41 parts by weight of N,N-dimethylformamide);
[0105] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 67° C., the nano-modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1100 r / min, and the modified resin was prepared after stirring for 4.45 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 192 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0106] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0107] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0108] Embodiment 11:
[0109] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0110] a. Ingredients: prepare 100 parts by weight of polyimide resin, 25 parts by weight of silicone resin, nano-modifier (3 parts by weight of hollow glass microspheres and 20 parts by weight of fumed silica), modification agent (0.022 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.067 parts by weight of 3-aminopropyltriethoxysilane), accelerator (0.04 parts by weight of imidazole and 0.004 parts by weight of diaminodiphenylmethane) and solvent (90 parts by weight of acetone and 45 parts by weight of butanone);
[0111] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 63° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1300 r / min, and the modified resin was prepared after stirring for 3.75 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 211 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0112] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0113] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0114] Embodiment 12:
[0115] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0116] a. Ingredients: prepare 100 parts by weight of polyimide resin, 30 parts by weight of silicone resin, nano-modifier (12 parts by weight of hollow glass microspheres and 8 parts by weight of fumed silica), modification agent (0.008 parts by weight of 3-aminopropyltriethoxysilane and 0.071 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.024 parts by weight of diaminodiphenylmethane and 0.017 parts by weight of boron trifluoride ethylamine) and solvent (62 parts by weight of acetone and 82 parts by weight of N,N-dimethylformamide);
[0117] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 54° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1450 r / min, and the modified resin was prepared after stirring for 4.15 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 268 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0118] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0119] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0120] Embodiment 13:
[0121] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0122] a. Ingredients: prepare 100 parts by weight of polyimide resin, 27 parts by weight of silicone resin, nano-modifier (19 parts by weight of fumed silica and 6 parts by weight of hollow glass microspheres), modification agent (0.019 parts by weight of 3-aminopropyltriethoxysilane and 0.077 parts by weight of γ-aminopropyltriethoxysilane), accelerator (0.037 parts by weight of boron trifluoride ethylamine and 0.016 parts by weight of diaminodiphenylmethane) and solvent (52 parts by weight of butanone, 52 parts by weight of acetone and 52 parts by weight of N,N-dimethylformamide);
[0123] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 74° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1350 r / min, and the modified resin was prepared after stirring for 4.45 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 226 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0124] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0125] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0126] Embodiment 14:
[0127] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0128] a. Ingredients: prepare 100 parts by weight of polyimide resin, 33 parts by weight of silicone resin, nano-modifier (9.5 parts by weight of hollow glass microspheres and 17.5 parts by weight of fumed silica), modification agent (0.054 parts by weight of γ-aminopropyltriethoxysilane and 0.061 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.034 parts by weight of boron trifluoride ethylamine and 0.023 parts by weight of imidazole) and solvent (28 parts by weight of butanone, 48 parts by weight of acetone and 91 parts by weight of N,N-dimethylformamide);
[0129] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 80° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin are stirred and mixed at a speed of 1400 r / min, and the modified resin is prepared after stirring for 5 hours for standby use. After cooling to room temperature, the solvent and the accelerator are added and stirred and mixed. The resin molding time is tested to be 300 s at 180° C., and the modified polyimide thermal insulation resin adhesive is obtained;
[0130] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0131] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0132] Embodiment 15:
[0133] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0134] a. Ingredients: prepare 100 parts by weight of polyimide resin, 31 parts by weight of silicone resin, nano-modifier (18 parts by weight of fumed silica and 12 parts by weight of hollow glass microspheres), modification treatment agent (0.038 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.075 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.035 parts by weight of imidazole and 0.03 parts by weight of diaminodiphenylmethane) and solvent (48 parts by weight of butanone, 72 parts by weight of acetone and 53 parts by weight of N,N-dimethylformamide);
[0135] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 85° C., the nano-modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1500 r / min, and the modified resin was prepared after stirring for 3.25 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 225 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0136] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0137] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0138] Embodiment 16:
[0139] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0140] a. Ingredients: prepare 100 parts by weight of polyimide resin, 35 parts by weight of silicone resin, nano-modifier (11 parts by weight of fumed silica and 20 parts by weight of hollow glass microspheres), modifying agent (0.024 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.095 parts by weight of γ-aminopropyltriethoxysilane), accelerator (0.05 parts by weight of imidazole and 0.023 parts by weight of diaminodiphenylmethane) and solvent (81 parts by weight of butanone, 62 parts by weight of acetone and 46 parts by weight of N,N-dimethylformamide);
[0141] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 83° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1350 r / min, and the modified resin was prepared after stirring for 4.65 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 234 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0142] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0143] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0144] Embodiment 17:
[0145] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0146] a. Ingredients: prepare 100 parts by weight of polyimide resin, 32 parts by weight of silicone resin, nano-modifier (17 parts by weight of hollow glass microspheres and 17 parts by weight of fumed silica), modification treatment agent (0.03 parts by weight of 3-aminopropyltriethoxysilane, 0.05 parts by weight of 3-glycidyloxypropyltrimethoxysilane and 0.05 parts by weight of γ-aminopropyltriethoxysilane), accelerator (0.041 parts by weight of boron trifluoride ethylamine and 0.041 parts by weight of diaminodiphenylmethane) and solvent (61 parts by weight of butanone, 32 parts by weight of acetone and 107 parts by weight of N,N-dimethylformamide);
[0147] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 76° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1450 r / min, and the modified resin was prepared after stirring for 4.15 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 276 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0148] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0149] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0150] Embodiment 18:
[0151] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0152] a. Ingredients: prepare 100 parts by weight of polyimide resin, 30 parts by weight of silicone resin, nano modifier (15 parts by weight of fumed silica and 20 parts by weight of hollow glass microspheres), modification treatment agent (0.016 parts by weight of 3-glycidyloxypropyltrimethoxysilane, 0.014 parts by weight of γ-aminopropyltriethoxysilane and 0.091 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.03 parts by weight of boron trifluoride ethylamine and 0.07 parts by weight of imidazole) and solvent (28 parts by weight of butanone, 75 parts by weight of acetone and 91 parts by weight of N,N-dimethylformamide);
[0153] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 73° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1250 r / min, and the modified resin was prepared after stirring for 3.75 hours for standby use. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested to be 291 s at 180° C., and the modified polyimide thermal insulation resin adhesive was obtained;
[0154] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0155] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and a lightweight polyimide insulation board is obtained.
[0156] Embodiment 19:
[0157] A method for preparing a lightweight polyimide insulation board comprises the following steps:
[0158] a. Ingredients: prepare 100 parts by weight of polyimide resin, 34 parts by weight of silicone resin, nano modifier (13 parts by weight of fumed silica and 19 parts by weight of hollow glass microspheres), modifying agent (0.044 parts by weight of γ-aminopropyltriethoxysilane, 0.024 parts by weight of 3-glycidyloxypropyltrimethoxysilane, 0.051 parts by weight of 3-aminopropyltriethoxysilane and 0.006 parts by weight of γ-glycidyloxypropyltrimethoxysilane), accelerator (0.019 parts by weight of imidazole, 0.073 parts by weight of boron trifluoride ethylamine and 0.004 parts by weight of diaminodiphenylmethane) and solvent (61 parts by weight of butanone, 43 parts by weight of acetone and 93 parts by weight of N,N-dimethylformamide);
[0159] b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 65° C., the nano modifier, the modifying agent, the polyimide resin and the silicone resin were stirred and mixed at a speed of 1400 r / min, and the modified resin was prepared after stirring for 4.5 hours. After cooling to room temperature, the solvent and the accelerator were added and stirred and mixed. The resin molding time was tested at 180° C. for 150 seconds, and the modified polyimide thermal insulation resin adhesive was obtained;
[0160] c. Preparation of modified polyimide thermal insulation resin fiber fabric prepreg: The modified polyimide thermal insulation resin adhesive prepared in step b is coated on the aramid fiber fabric through a gluing machine, and then the aramid fiber fabric coated with the modified polyimide thermal insulation resin adhesive is placed in a drying tunnel, wherein the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, and the baking temperature range is 100℃~185℃, wherein: the first section is 105℃~125℃, the second section is 135℃~165℃, the third section is 165℃~185℃, and the fourth section is 100℃~110℃. The speed of the gluing machine is 10m / min~25m / min, and the modified polyimide thermal insulation resin fiber fabric prepreg is obtained. The drying tunnel is pre-baked before baking. The soluble resin content of the fiber fabric prepreg is greater than or equal to 95%, and the volatile matter is less than or equal to 2%; the specific process parameters are shown in Table 1;
[0161] d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, and after closing the mold, perform hot pressing molding at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa. The hot pressing time is 0.5h to 50h. The specific process parameters are shown in Table 2, and the lightweight polyimide insulation board is obtained.
[0162] The specific process parameters of Examples 1 to 19 and the technical performance test results of the lightweight polyimide insulation board are shown in Tables 1, 2 and 3 below respectively:
[0163] Table 1: Example modified polyimide thermal insulation resin fiber fabric prepreg preparation process parameters and central control technical indicators
[0164]
[0165]
[0166] Table 2: Lightweight polyimide insulation board pressing process parameters
[0167]
[0168]
[0169] Table 3: Technical performance test data of lightweight polyimide insulation boards prepared in Examples 1-19
[0170]
[0171]
[0172] As shown in Table 1 and Table 2, the lightweight polyimide insulation board of the present invention has a bending strength of 380MPa-450MPa at room temperature, a bending strength of 267MPa-331MPa at 180°C, a tensile strength of 365MPa-387MPa, and a notched impact strength of 60KJ / m 2 ~70KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m·k and density is 1.55g / cm 3 ~1.75g / cm 3 , especially suitable for use in the field of lightweight insulation.
[0173] Embodiment 20:
[0174] A lightweight polyimide heat insulation board, which is a lightweight polyimide heat insulation board made by hot pressing multiple layers of overlapping modified polyimide heat insulation resin fiber fabric prepreg (the number of layers of the modified polyimide heat insulation resin fiber fabric prepreg is not limited and can be any one of 1-500 layers as required);
[0175] The modified polyimide thermal insulation resin fiber fabric prepreg is obtained by coating the modified polyimide thermal insulation resin adhesive on the aramid fiber fabric and then baking;
[0176] The modified polyimide heat-insulating resin adhesive is composed of 100 parts by weight of polyimide resin, 35 parts by weight of silicone resin, 35 parts by weight of nano-modifier, 0.13 parts by weight of modification treatment agent, 0.1 parts by weight of accelerator and 200 parts by weight of solvent;
[0177] The aramid fiber fabric is any one of aramid fiber plain cloth, aramid fiber twill cloth, aramid fiber gingham cloth, aramid fiber multi-axial cloth and aramid fiber composite cloth.
[0178] Embodiment 21:
[0179] A lightweight polyimide heat insulation board, which is a lightweight polyimide heat insulation board made by hot pressing multiple layers of overlapping modified polyimide heat insulation resin fiber fabric prepreg (the number of layers of the modified polyimide heat insulation resin fiber fabric prepreg is not limited and can be any one of 1-500 layers as required);
[0180] The modified polyimide thermal insulation resin fiber fabric prepreg is obtained by coating the modified polyimide thermal insulation resin adhesive on the aramid fiber fabric and then baking;
[0181] The modified polyimide heat-insulating resin adhesive is composed of 100 parts by weight of polyimide resin, 15 parts by weight of silicone resin, 5 parts by weight of nano-modifier, 0.04 parts by weight of modification treatment agent, 0.005 parts by weight of accelerator and 50 parts by weight of solvent;
[0182] The aramid fiber fabric is any one of aramid fiber plain cloth, aramid fiber twill cloth, aramid fiber gingham cloth, aramid fiber multi-axial cloth and aramid fiber composite cloth.
[0183] Embodiment 22:
[0184] A lightweight polyimide heat insulation board, which is a lightweight polyimide heat insulation board made by hot pressing multiple layers of overlapping modified polyimide heat insulation resin fiber fabric prepreg (the number of layers of the modified polyimide heat insulation resin fiber fabric prepreg is not limited and can be any one of 1-500 layers as required);
[0185] The modified polyimide thermal insulation resin fiber fabric prepreg is obtained by coating the modified polyimide thermal insulation resin adhesive on the aramid fiber fabric and then baking;
[0186] The modified polyimide thermal insulation resin adhesive is composed of 100 parts by weight of polyimide resin, 25 parts by weight of silicone resin, 20 parts by weight of nano-modifier, 0.085 parts by weight of modification treatment agent, 0.053 parts by weight of accelerator and 130 parts by weight of solvent;
[0187] The aramid fiber fabric is any one of aramid fiber plain cloth, aramid fiber twill cloth, aramid fiber gingham cloth, aramid fiber multi-axial cloth and aramid fiber composite cloth.
[0188] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
[0189] In the above embodiments: the percentages used, unless otherwise specified, are all weight (mass) percentages or percentages known to those skilled in the art; the proportions used, unless otherwise specified, are all weight (mass) proportions; and the weights may be in grams or kilograms.
[0190] In the above embodiments, the process parameters (temperature, pressure, time, vehicle speed, rotation speed, etc.) and the amount of each component in each step are ranges, and any point can be applied.
[0191] The technical contents not specifically described in the present invention and the above embodiments are the same as the prior art, and the raw materials are all commercially available products.
[0192] The present invention is not limited to the above embodiments, and all of the contents of the present invention can be implemented and have the above good effects.
Claims
1. A lightweight polyimide insulation board, characterized by: The lightweight polyimide heat insulation board is a lightweight polyimide heat insulation board made by hot pressing multiple layers of overlapping modified polyimide heat insulation resin fiber fabric prepreg; The modified polyimide thermal insulation resin fiber fabric prepreg is obtained by coating the modified polyimide thermal insulation resin adhesive on the aramid fiber fabric and then baking; The modified polyimide heat-insulating resin adhesive is composed of 100 parts by weight of polyimide resin, 15 to 35 parts by weight of silicone resin, 5 to 35 parts by weight of nano-modifier, 0.04 to 0.13 parts by weight of modification treatment agent, 0.005 to 0.1 parts by weight of accelerator and 50 to 200 parts by weight of solvent; The aramid fiber fabric is at least one of aramid fiber plain cloth, aramid fiber twill cloth, aramid fiber gingham cloth, aramid fiber multi-axial cloth and aramid fiber composite cloth.
2. The lightweight polyimide thermal insulation board according to claim 1, characterized in that: In the modified polyimide thermal insulation resin adhesive: The nano modifier is one or a mixture of fumed silica and hollow glass microspheres; The modifying agent is any one of 3-aminopropyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyloxypropyl trimethoxysilane, or a mixture of two or more thereof; The accelerator is any one of imidazole, diaminodiphenylmethane, and boron trifluoride ethylamine, or a mixture of two or more thereof; The solvent is any two of acetone, butanone, and N,N-dimethylformamide or a mixture of two or more thereof.
3. The lightweight polyimide thermal insulation board according to claim 1 or 2, characterized in that: The hot pressing molding is: after preheating the template at 145°C to 175°C, the modified polyimide insulation resin fiber fabric prepreg is overlapped and placed in the template, and after closing the mold, hot pressing molding is performed under the conditions of temperature 210°C to 220°C and pressure 1MPa to 25MPa, and the hot pressing time is 0.5h to 50h.
4. The lightweight polyimide thermal insulation board according to claim 1 or 2, characterized in that: The baking is as follows: placing the aramid fiber fabric coated with the modified polyimide heat-insulating resin adhesive into a drying tunnel, the drying tunnel is 50 meters long and is divided into 4 sections, each section is 12.5 meters long, the baking temperature ranges from 100°C to 185°C, wherein: the first section is 105°C to 125°C, the second section is 135°C to 165°C, the third section is 165°C to 185°C, and the fourth section is 100°C to 110°C, and the speed of the gluing machine is 10m / min to 25m / min.
5. The lightweight polyimide thermal insulation board according to claim 1 or 2, characterized in that: The preparation method of the modified polyimide thermal insulation resin adhesive is as follows: at a temperature of 50°C to 85°C, the nano-modifier, the modification treatment agent, the polyimide resin and the silicone resin are stirred and mixed at a speed of 800r / min to 1500r / min, and after stirring for 3h to 5h, a modified resin is prepared for standby use, and after cooling to room temperature, a solvent and a promoter are added and stirred to obtain the modified polyimide thermal insulation resin adhesive.
6. The lightweight polyimide heat insulation board according to claim 1 or 2, characterized in that: In the modified polyimide thermal insulation resin fiber fabric prepreg, the weight percentage of the modified polyimide thermal insulation resin adhesive is 30% to 50%, and the weight percentage of the aramid fiber fabric is 50% to 70%.
7. A method for preparing a lightweight polyimide insulation board, characterized in that The following steps are involved: a. Ingredients: prepare the raw materials of each component according to the ratio of 100 parts by weight of polyimide resin, 15-35 parts by weight of silicone resin, 5-35 parts by weight of nano modifier, 0.04-0.13 parts by weight of modification treatment agent, 0.005-0.1 parts by weight of accelerator and 50-200 parts by weight of solvent; b. Preparation of modified polyimide thermal insulation resin adhesive: at a temperature of 50° C. to 85° C., the nano-modifier, the modifying agent, the polyimide resin and the silicone resin are stirred and mixed at a speed of 800 r / min to 1500 r / min, and stirred for 3 h to 5 h to prepare a modified resin for standby use. After cooling to room temperature, a solvent and a accelerator are added and stirred to obtain a modified polyimide thermal insulation resin adhesive; c. Preparing a modified polyimide thermal insulation resin fiber fabric prepreg: coating the modified polyimide thermal insulation resin adhesive prepared in step b on the aramid fiber fabric, and then baking to obtain the modified polyimide thermal insulation resin fiber fabric prepreg; The aramid fiber fabric is at least one of aramid fiber plain fabric, aramid fiber twill fabric, aramid fiber gingham fabric, aramid fiber multiaxial fabric, and aramid fiber composite fabric; d. Preparation of lightweight polyimide insulation board: preheat the template at 145°C to 175°C, overlap the modified polyimide insulation resin fiber fabric prepreg and place it in the template, close the mold and perform hot pressing at a temperature of 210°C to 220°C and a pressure of 1MPa to 25MPa for 0.5h to 50h to obtain a lightweight polyimide insulation board.
8. The method for preparing the lightweight polyimide heat insulation board according to claim 7, characterized in that: The baking is to put the aramid fiber fabric coated with modified polyimide thermal insulation resin adhesive into a drying tunnel, the drying tunnel is 50m long and divided into 4 sections, each section is 12.5m, the baking temperature range is 100°C to 185°C, wherein: the first section is 105°C to 125°C, the second section is 135°C to 165°C, the third section is 165°C to 185°C, and the fourth section is 100°C to 110°C, and the speed of the gluing machine is 10m / min to 25m / min.
9. The method for preparing the lightweight polyimide heat insulation board according to claim 7 or 8, characterized in that: Ingredients in step a: The nano modifier is one or a mixture of fumed silica and hollow glass microspheres; The modifying agent is any one of 3-aminopropyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyloxypropyl trimethoxysilane, or a mixture of two or more thereof; The accelerator is any one of imidazole, diaminodiphenylmethane, and boron trifluoride ethylamine, or a mixture of two or more thereof; The solvent is any two of acetone, butanone, and N,N-dimethylformamide or a mixture of two or more thereof.
10. The method for preparing the lightweight polyimide heat insulation board according to claim 7 or 8, characterized in that: The performance parameters of the obtained lightweight polyimide insulation board are: bending strength at room temperature is 380MPa ~ 450MPa, flexural strength at 180°C 267MPa ~ 331MPa, tensile strength 365MPa~387MPa, notched impact strength 60KJ / m 2 ~ 70KJ / m 2 , Insulation resistance greater than or equal to 10 8 MΩ, flame retardancy reaches UL94 V-0 level, thermal conductivity (25℃) is less than 0.2w / m•k, density is 1.55g / cm 3 ~1.75g / cm 3 .
Citation Information
Patent Citations
Light / high-temperature-resistant integrated composite material satellite light shield and preparation method thereof
CN113911401A
Polyimide / inorganic nano-composite laminated board and its preparation method
CN1718428A
Prepreg and fiber-reinforced plastic
JP1995041577A
Modified bismaleimide prepolymer, preparation method therefor, and application thereof
US20240043595A1