Anti-warping low-temperature-resistant continuous fiber reinforced thermoplastic resin and preparation method thereof
By adding the first resin and its derived elastomer second resin to the continuous fiber reinforced thermoplastic resin to form an island structure, the problem of insufficient warping and low-temperature impact resistance is solved, and the excellent mechanical properties and low-cost preparation of the material are achieved.
Patent Information
- Application Number
- CN202410998061.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Continuous fiber-reinforced thermoplastic composites are prone to warping due to shrinkage differences and resin crystallinity during the preparation process, and they are insufficient impact resistance under low temperature environments.
Using a warpage-resistant and low-temperature-resistant continuous fiber-reinforced thermoplastic resin including a matrix resin and a continuous fiber, the low crystallinity and elastic structure of the second resin are utilized by adding a first resin and a second resin derived thereto to the matrix resin. The shrinkage of the first resin is restrained, an island structure is formed to improve toughness, and a material with excellent mechanical properties is prepared by a specific molding process.
It effectively solves the warping problem, improves impact and shock resistance at low temperatures, enhances the flexibility and fatigue resistance of the material, and does not require additional compatibilizers, which are simple to operate and low cost.
Smart Images

Figure BDA0004960817260000041 
Figure BDA0004960817260000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of continuous fiber reinforced thermoplastic composite materials, and in particular relates to a warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin and a preparation method thereof. Background Art
[0002] In recent years, continuous fiber reinforced thermoplastic composites have been widely used in the fields of automobiles, electronic appliances, etc. as materials that are both lightweight and rigid. This type of fiber reinforced composite material is generally made of a matrix resin made of polypropylene or nylon reinforced by reinforcing fibers such as glass fiber, carbon fiber or aramid fiber. Many reinforced fiber composite materials on the market are mostly made in two ways: one is to prepare complex devices or sheets by laminating a single-layer composite prepreg; the other is to make it by spreading the resin film and the fiber interlayer and heating and molding. These reinforced fiber composite materials have high modulus and strength, so they can replace many metal parts. As the market trend is moving towards reducing the weight of products, more and more products are achieving lightweight substitution, but in the process of product preparation, more and more problems are revealed.
[0003] Stability of the parts (no warping: the main problem of these hard materials obtained by adding glass fibers). During the cycle time of industrial products, the products are demoulded before they are completely cooled. Warping is caused by internal constraints, and the result (or relaxation) is deformation of the parts. For these continuous fiber reinforced materials, the orientation of the fibers is fixed, and the fiber ply structure of most products is anisotropic due to the different forces on the products. The orientation of the fibers has the result of limiting the shrinkage in this direction. On the contrary, in the direction perpendicular to the fiber axis, the shrinkage rate is controlled by the polymer, so the shrinkage is greater, which is the main reason for the warping caused by the shrinkage difference. The second is that the crystallinity of the resin causes overall shrinkage, which is obvious for polymers reinforced with high glass fiber content. Therefore, it is necessary to develop a thermoplastic resin that is anti-warping, resistant to low temperatures, and has excellent comprehensive mechanical properties, which is of great significance to this field. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin and a preparation method thereof.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A warping-resistant and low-temperature-resistant continuous fiber-reinforced thermoplastic resin, comprising a matrix resin and continuous fibers;
[0007] The matrix resin comprises a first resin and a second resin, wherein the first resin is a thermoplastic resin; the second resin is an elastomer derived from the first resin; and the mass ratio of the first resin to the second resin is 50-90:10-50;
[0008] The mass proportion of the continuous fibers in the anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin is 50-80%.
[0009] The second resin is a derivative elastomer of the first resin and has an island effect or a co-continuous structure, which makes the first resin and the second resin have some of the same components in the molecular chain. The two can be well compatible and will not peel off from each other. The first resin crystallizes quickly and has a high degree of crystallinity. After cooling, it is easier to shrink. The second resin crystallizes slowly and has a lower degree of crystallinity, which restrains the shrinkage of the first resin. After molding, the shrinkage deformation is smaller and no warping occurs. Because the second resin has a crystallization speed that is the same as the first resin elastomer, the shrinkage rate is relatively lower, and the surface of the continuous fiber sheet will not shrink, resulting in fiber exposure, and has a better appearance.
[0010] The second resin is an elastomeric structure, which is polymerized from the hard segment of the first resin and the soft segment of the second resin. Microphase separation will occur at the molecular microscopic level to form an island structure, that is, a structure in which one phase (island phase) is discontinuously mixed in another phase (sea phase) and looks relatively continuous, or a structure in which one phase looks relatively continuous. It can absorb impact energy and make the sheet have better toughness. The second monomer is an elastomer and has two glass transition temperatures, of which the α transition temperature is basically the same as that of the first resin, and the β transition temperature is generally the transition temperature of the continuous phase glass, of which the β transition temperature is lower than -50°C, so that the anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin of the present invention can have good impact resistance in low-cold areas.
[0011] The above-mentioned anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin, preferably, the first resin includes any one or more of polyamide, polyester, polyphenylene sulfide, polyphenylene ether, polycarbonate, polyether ketone, polysulfide ether ketone, polyether ether ketone, polyethylene, polypropylene and polystyrene. More preferably, polyamide, polycarbonate and polypropylene.
[0012] In the above-mentioned anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin, preferably, the second resin is any one or more of polyamide elastomer, polyester elastomer and ethylene propylene diene monomer rubber.
[0013] The second resin is a block copolymer with a glass transition temperature lower than room temperature, and part of the molecules are constrained by ionic bonds, van der Waals forces or molecular chain entanglement; and the second resin has the same components as the first resin, and the mass percentage of the same components in the second resin exceeds 50%. The above elastomers meet the above requirements for the second resin.
[0014] More preferably, the first resin is nylon 6 (PA6), and the second resin is nylon 6 elastomer (TPAE), wherein the nylon 6 elastomer is a copolymer of nylon 6 and terminal hydroxyl polytetramethylene ether (PTMG), containing 50% of PTMG components.
[0015] More preferably, the first resin is polyester (PET), and the second resin is polyester elastomer (TPEE), wherein the polyester elastomer is a copolymer of polyester and terminal hydroxyl polytetramethylene ether (PTMG), containing 50% of PTMG component.
[0016] More preferably, the first resin is polypropylene (PP), and the second resin is ethylene propylene diene monomer (EPDM), wherein the EPDM elastomer is made by copolymerization of ethylene, propylene and non-conjugated diene monomers, and contains 60% propylene components.
[0017] In the present invention, the first resin is a homopolymer resin (such as nylon 6 is polycaprolactam), and the second resin is a copolymer resin (such as obtained by copolymerizing polycaprolactam and polyether). From a macroscopic perspective, the first and second resins are both nylons, and the two are compatible and will not separate. From a microscopic perspective, the second resin is obtained by polymerizing two parts, wherein the nylon 6 part will crystallize to produce an island structure, while the polyether part will not crystallize and is a soft sea structure, so when an impact occurs, the soft sea structure part will absorb energy, that is, microphase separation, and it has both the rigidity of an island and can withstand impact.
[0018] The above-mentioned anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin, preferably, the continuous fiber is a fiber cloth formed by weaving or knitting any one or more fibers of glass fiber, carbon fiber, basalt fiber and aramid fiber.
[0019] In the above-mentioned anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin, preferably, the continuous fiber is a continuous fiber surface-treated with a coupling agent; the coupling agent is a silane coupling agent.
[0020] The above-mentioned warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin, preferably, does not require a compatibilizer.
[0021] Based on a general inventive concept, the present invention also provides a method for preparing a warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin, comprising the following steps:
[0022] (1) Shearing and plasticizing the first resin and the second resin respectively, and casting and pultruding them into micron-level films to obtain a first resin film and a second resin film;
[0023] (2) weaving or knitting continuous glass fibers into cloth, performing surface treatment with a coupling agent, and performing dehydration treatment to obtain a fiber cloth;
[0024] (3) alternately layering the first resin film obtained in step (1), the second resin film, and the fiber cloth obtained in step (2) in a predetermined order;
[0025] (4) Molding the layer obtained in step (3) to obtain the anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin.
[0026] In the above-mentioned preparation method, preferably, in step (1), the thickness of the first resin film and the second resin film is 60-100 μm; in step (2), the dehydration treatment is a dehydration hot air baking dehydration treatment at 120-180°C for 1-4 hours.
[0027] Preferably, in step (3), the second resin film is evenly distributed in the laminate; in step (4), the molding conditions are as follows: preheating temperature: 220-235°C, pressure 200kg / cm 2 ; Hot pressing temperature 240-280℃, pressure 350kg / cm 2 ; Cooling temperature 40-60℃, pressure 350kg / cm 2 , molding speed 0.20-2m / min.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin of the present invention solves the problem of easy warping during the production process of products, while improving the low-temperature impact resistance at -50°C and improving the seismic resistance of the composite material.
[0030] 2. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin of the present invention has good flexibility, can fully cope with various working conditions of the product, and increases the fatigue resistance of the product; no additional auxiliary reagents, such as a compatibilizer, are required.
[0031] 3. The preparation method of the present invention is simple to operate and can be produced using existing equipment at a low cost. DETAILED DESCRIPTION
[0032] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in combination with the specification and preferred embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.
[0033] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0035] Example:
[0036] The invention discloses a warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin, wherein the continuous glass fiber cloth is selected with a warp and weft yarn density of 2400TEX and a gram weight of 800g / m 2 The plain yarn is treated with a silane coupling agent before use.
[0037] In an embodiment of the present invention, the first resin is nylon 6 (PA6), and the second resin is nylon 6 elastomer (TPAE), wherein the nylon 6 elastomer is a copolymer of nylon 6 and terminal hydroxyl polytetramethylene ether (PTMG), containing 50% of PTMG components.
[0038] In the embodiment of the present invention, the first resin may also be polyester (PET), and the second resin is polyester elastomer (TPEE), wherein the polyester elastomer is a copolymer of polyester and terminal hydroxyl polytetramethylene ether (PTMG) and contains 50% PTMG component.
[0039] In an embodiment of the present invention, the first resin may also be polypropylene (PP), and the second resin is ethylene propylene diene monomer (EPDM), wherein the EPDM elastomer is made by copolymerization of ethylene, propylene and non-conjugated diene monomers and contains 60% propylene components.
[0040] The specific formulas of Examples 1-9 of the present invention are shown in Table 1.
[0041] Table 1 Example formula table
[0042]
[0043] The preparation method of the present invention comprises the following steps: the resins are respectively sheared and plasticized by a screw extruder, and then cast and extruded into a film with a thickness of 70um and a width of 1300mm; the continuous glass fiber is surface treated, and then subjected to a hot air baking and dehydration treatment at 150°C for 4 hours; the glass fiber fabric, the first resin film and the second resin film are layered alternately with the glass fiber fabric and the resin in a predetermined order by a laying device, and the layering sequence is designed according to the proportion of the second resin so that the second resin is evenly layered in the plate. Then, the laying, automatic edge alignment, positioning and unwinding are performed to obtain a layer of glass fiber fabric and resin film. The layer is introduced into the molding equipment, and the preheating temperature is: 220-235°C, and the pressure is 200kg / cm 2 ; Hot pressing temperature 240-280℃, pressure 350kg / cm 2; Cooling temperature 40-60℃, pressure 350kg / cm 2 , molding speed 0.10m / min, and a long continuous glass fiber reinforced polyamide composite material with a thickness of 3mm was prepared.
[0044] Warping test: Place a 1m*1m plate on a marble horizontal platform and calculate the warping amount.
[0045] The properties of Examples 1-9 of the present invention are shown in Table 2.
[0046] Table 2 Performance table of the embodiment
[0047]
[0048] In general, the present invention adds an elastic component derived from the first resin to the anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin, and the various components have good compatibility, which solves the problem of easy warping during the production process of the product, while improving the low-temperature impact resistance at -50°C and the shock resistance of the continuous fiber reinforced thermoplastic resin.
Claims
1. A warping-resistant low-temperature-resistant continuous fiber reinforced thermoplastic resin, characterized in that: including a matrix resin and continuous fibers; The matrix resin comprises a first resin and a second resin, wherein the first resin is a thermoplastic resin; the second resin is an elastomer derived from the first resin; and the mass ratio of the first resin to the second resin is 50-90:10-50; The mass proportion of the continuous fibers in the anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin is 50-80%.
2. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to claim 1, characterized in that: The first resin includes any one or more of polyamide, polyester, polyphenylene sulfide, polyphenylene ether, polycarbonate, polyether ketone, polysulfide ether ketone, polyether ether ketone, polyethylene, polypropylene and polystyrene.
3. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to claim 2, characterized in that: The second resin is any one or more of polyamide elastomer, polyester elastomer and EPDM rubber.
4. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to claim 3, characterized in that: The first resin and the second resin are any combination of the following: The first resin is nylon 6, and the second resin is nylon 6 elastomer; The first resin is polyester, and the second resin is a polyester elastomer; The first resin is polypropylene, and the second resin is ethylene propylene diene monomer rubber.
5. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to claim 1, characterized in that: The continuous fibers are fiber cloths formed by weaving or knitting any one or more of glass fibers, carbon fibers, basalt fibers and aramid fibers.
6. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to claim 5, characterized in that: The continuous fiber is a continuous fiber that has been surface treated with a coupling agent; the coupling agent is a silane coupling agent.
7. The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to any one of claims 1 to 6, characterized in that: The anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin does not require a compatibilizer.
8. A method for preparing the anti-warping low-temperature resistant continuous fiber reinforced thermoplastic resin according to any one of claims 1 to 7, characterized in that: The steps include: (1) Shearing and plasticizing the first resin and the second resin respectively, and casting and pultruding them into micron-level films to obtain a first resin film and a second resin film; (2) weaving or knitting continuous glass fibers into cloth, performing surface treatment with a coupling agent, and performing dehydration treatment to obtain a fiber cloth; (3) alternately layering the first resin film obtained in step (1), the second resin film, and the fiber cloth obtained in step (2) in a predetermined order; (4) Molding the layer obtained in step (3) to obtain the anti-warping and low-temperature resistant continuous fiber reinforced thermoplastic resin.
9. The preparation method according to claim 8, characterized in that: In step (1), the thickness of the first resin film and the second resin film is 60-100 μm; in step (2), the dehydration treatment is a dehydration hot air baking dehydration treatment at 120-180° C. for 1-4 hours.
10. The preparation method according to claim 8, characterized in that: In step (3), the second resin film is evenly distributed in the laminate; in step (4), the molding conditions are as follows: preheating temperature: 220-235°C, pressure 200-250kg / cm 2 ; Hot pressing temperature 240-280℃, pressure 350-400kg / cm 2 ; Cooling temperature 40-60℃, pressure 350-400kg / cm 2 , molding speed 0.20-2m / min.
Citation Information
Patent Citations
Preparation method of composite material by using fibers to improve strength of polypropylene
CN109705451A
Bonding resin for continuous fiber reinforced plastic composite pipe and preparation method thereof
CN109749663A
Continuous glass fiber reinforced thermoplastic composite material and preparation method thereof
CN111572059A
Prepreg for automatic fiber placement process and preparation method of prepreg
CN112300534A
Preparation method of long fiber reinforced sheet molding compound
CN117532918A