Method and device for preparing iron phosphate through precipitation conversion
Iron phosphate was prepared by precipitation conversion method, and rapid conversion was achieved using iron active hydroxide intermediates and low phosphorus source, which solved the problems of transfer crystals and high energy consumption in iron phosphate production, and improved the performance of iron phosphate and lithium battery. performance.
Patent Information
- Application Number
- CN202411025138.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-25
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
There are problems such as difficulty in crystallization, long crystallization time and large phosphoric acid consumption in the production process, resulting in increased costs and high energy consumption.
By using the precipitation conversion method, the sulfur content is reduced by preparing iron active hydroxide intermediates, and an additional excess of no more than 5% of the phosphorus source is used during the conversion process to achieve rapid conversion, reduce energy consumption and raw material usage, and improve the conversion rate.
It achieves rapid conversion, reduces production costs and energy consumption, improves the processing performance of iron phosphate and the high capacity and high rate performance of lithium batteries.
Smart Images

Figure CN118929596A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery materials, and in particular to a method and device for preparing iron phosphate through precipitation conversion. Background Art
[0002] With the rapid development of new energy vehicles and increasingly fierce competition in the industry, lithium iron phosphate batteries have occupied 70% of the electric vehicle market share due to their advantages of low cost, high safety and long cycle life. Among them, the precursor iron phosphate plays a major role in the physical and chemical properties of lithium iron phosphate. At present, my country's iron phosphate production capacity is about 3.7 million tons / year and the output is about 176,000 tons / month. The iron phosphate production technology faces challenges in cost, stability and performance control. The development of an iron phosphate preparation process with low cost, good processing performance and high batch stability is of great significance for reducing costs and increasing efficiency in the iron phosphate industry.
[0003] At present, the mainstream process for producing iron phosphate in the industry is the two-step co-precipitation method. The so-called two-step method means that in the first step, the iron salt is oxidized and the pH value is adjusted to prepare the iron phosphate intermediate - basic iron phosphate. In this way, most of the sulfur and impurities brought into the system by the iron source can be drawn out of the system through the synthetic mother liquor, and then the intermediate is slurried and washed to further reduce the impurities in the intermediate. The second step is to add the intermediate, phosphoric acid and water into the reaction vessel for stirring, and then heat it to a certain temperature for insulation conversion reaction to prepare dihydrate iron phosphate. After slurry washing and drying and sintering treatment, the anhydrous iron phosphate product is finally obtained. However, this method faces the following problems: (1) It is difficult to control the pH of the basic iron phosphate intermediate. When the pH is adjusted too high, it is difficult to convert the basic iron phosphate into iron phosphate when the phosphoric acid consumption remains unchanged; (2) In the conversion reaction, it is often necessary to add phosphoric acid with a higher unit consumption for crystal conversion, and the added phosphoric acid mainly acts as a conversion medium to adjust the pH value of the system so that the basic iron phosphate is converted into the crystal form of iron phosphate, resulting in excessive phosphoric acid consumption and increased costs. On the other hand, the reuse of the converted phosphoric acid mother liquor will cause impurities to accumulate in the system, which will have a negative impact on subsequent production; (3) During the conversion reaction, the speed of crystal conversion is often slow, generally 1 to 2 hours. After the crystal conversion is completed, it is still necessary to maintain a high temperature of more than 90°C for 1.5 to 2 hours, which consumes a lot of energy. The present invention provides a process for preparing iron phosphate by a precipitation conversion method with rapid crystal conversion and low phosphorus excess coefficient, aiming to reduce the problems of difficult crystal conversion, long crystal conversion time and large phosphorus source consumption in the production process of iron phosphate, which has important practical significance for reducing costs and increasing efficiency in the new energy industry. Summary of the invention
[0004] The present invention provides a method and device for preparing ferric phosphate by precipitation conversion, which can solve the problems of difficult crystal conversion and long crystal conversion time in the production process of ferric phosphate.
[0005] In order to solve the above technical problems, this application provides the following technical solutions: A method for preparing ferric phosphate by precipitation conversion comprises the following steps: S1: Dissolve the iron source in water or acid; S2: Add impurity remover, raise the temperature to 20-90°C, stir for 1-6 hours and then separate to obtain liquid A; S3: adding alkali solution to solution A to obtain an iron active hydroxide intermediate, wherein the amount of alkali solution added is 0.5% to 300% relative to the molar amount of iron; S4: pulping and washing the active iron hydroxide intermediate 1 to 4 times to obtain a filter cake; S5: dissolving the phosphorus source in water to obtain solution B; S6: drying and measuring the washed filter cake and adding it to the reactor, and adding 1 to 10 times the mass of water relative to the mass of the intermediate and 98% to 105% of the molar amount of the iron source in the iron active hydroxide intermediate to the reactor; S7: After stirring evenly, raise the temperature to 70-99°C and keep the temperature for 0.2-2h to obtain ferric phosphate dihydrate slurry; S8: The dihydrate ferric phosphate slurry is subjected to solid-liquid separation, washed 1-5 times, and then sintered at 450-700° C. for 1-6 hours to obtain anhydrous ferric phosphate.
[0006] Beneficial effects of this scheme: This scheme innovatively prepares an iron active hydroxide intermediate in the first step of the synthesis process, so that most of the anionic impurities brought into the iron source are introduced into the synthesis mother liquor during the synthesis process, fundamentally reducing the sulfur content in the product, and this active body is different from the intermediate of basic iron phosphate in the current production process, and is a brand-new intermediate with the characteristics of fine particle size, which will help to improve the conversion of iron phosphate and subsequent processing performance. In the conversion process, the iron active hydroxide intermediate provided by the present invention is used for conversion, and only an additional excess of no more than 5% of the phosphorus source is required, and the conversion can be completed within 0.5h under the ideal conversion temperature conditions. Compared with the existing process, the utilization rate of phosphate is high, and great progress has been made in reducing the amount of raw materials, energy consumption, increasing the conversion rate and reducing the production cost. The synthesized iron phosphate has a micro-sodium network structure of primary particles at the nanoscale, so that the lithium iron phosphate synthesized with this as the raw material has high capacity and high rate performance.
[0007] Further, the iron source in step S1 is one or more of ferroferric oxide, ferrous oxide, ferrous sulfate, ferrous chloride, ferrous nitrate, ferric sulfate, ferric chloride, and iron powder.
[0008] Furthermore, the iron source is trivalent iron.
[0009] Furthermore, the acid solution in step S1 includes one or more of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, and phosphoric acid solution.
[0010] Furthermore, the impurity remover in step S2 includes one or more of ammonia water, monoammonium dihydrogen phosphate, and iron powder.
[0011] Furthermore, the alkali solution in step S3 is one or more of sodium hydroxide solution, calcium hydroxide, ammonia solution, sodium carbonate solution, and potassium hydroxide solution.
[0012] Furthermore, the phosphorus source in step S5 is one or more of monoammonium phosphate, diammonium phosphate, triammonium phosphate, and phosphoric acid.
[0013] A device for preparing ferric phosphate by precipitation conversion, comprising: A base; a stirring cylinder is arranged on the base; Heating resistor: set in the inner wall of the mixing tank, used to control the heating temperature of the liquid in the mixing tank; Lifting cylinder: The restraining end of the lifting cylinder is fixed on the base, and the cylinder shaft end of the lifting cylinder extending out of the cylinder is fixed to the frame; Motor: The restraining end of the motor is fixed on the frame, and the rotating shaft of the motor extends into the mixing tank; Feeding plate: arranged at the opening above the mixing tank, the feeding plate is coaxially fixed with the rotating shaft; Feed pipe: a plurality of leakage holes are evenly spaced at the bottom of the feeding plate, each leakage hole is connected to a feed pipe; the feed pipe is parallel to the rotating shaft; the rotating shaft is fixedly connected to the feed pipe through a cross bar; Stirring blade: The stirring blade is connected with the material passing pipe; a nozzle is arranged at the end of the stirring blade.
[0014] The basic principles and beneficial effects of this solution: the setting of the heating resistor can stably maintain the temperature in the stirring tank and adjust it to the temperature required for the reaction; the motor shaft is integrated with the feeding plate, the feeding pipe and the stirring fan blades. At the end of the reaction, the lifting cylinder is started and the cylinder shaft moves upward, which can lift the shaft upward, so that there is no other structure in the stirring tank, which is convenient for subsequent processing of the liquid in the tank; this solution can realize the slow addition of reactants, avoiding the problem of poor reaction effect caused by excessive addition at one time. At the same time, adding materials according to the stirring rhythm can make the newly added raw materials fully contact with the reactants, improve the reaction efficiency and save reaction time. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a SEM image of the iron phosphate prepared in Example 1.
[0016] Figure 2 This is the XRD pattern of the iron phosphate prepared in Example 1.
[0017] Figure 3 This is a charge and discharge curve diagram of the lithium iron phosphate prepared in Example 1.
[0018] Figure 4 This is the cycle diagram of the lithium iron phosphate prepared in Example 1.
[0019] Figure 5 This is the high rate performance curve of the lithium iron phosphate prepared in Example 1.
[0020] Figure 6 Schematic diagram of the device structure for preparing iron phosphate by precipitation conversion.
[0021] The accompanying drawings in the specification are as follows: base 1, lifting cylinder 2, cylinder shaft 3, frame 4, motor 5, rotating shaft 6, feeding tray 7, feeding pipe 8, stirring blade 9, heating resistor 10. DETAILED DESCRIPTION
[0022] The following is further described in detail through specific implementation methods: A method for preparing ferric phosphate by precipitation conversion comprises the following steps: S1: Dissolve the iron source in water or acid; S2: Add impurity remover, raise the temperature to 20-90°C, stir for 1-6 hours and then separate to obtain liquid A; S3: adding alkali solution to solution A to obtain an iron active hydroxide intermediate, wherein the amount of alkali solution added is 0.5% to 300% relative to the molar amount of iron; S4: pulping and washing the active iron hydroxide intermediate 1 to 4 times to obtain a filter cake; S5: dissolving the phosphorus source in water to obtain solution B; S6: drying and measuring the washed filter cake and adding it to the reactor, and adding 1 to 10 times the mass of water relative to the mass of the intermediate and 98% to 105% of the molar amount of the iron source in the iron active hydroxide intermediate to the reactor; S7: After stirring evenly, raise the temperature to 70-99°C and keep the temperature for 0.2-2h to obtain ferric phosphate dihydrate slurry; S8: The dihydrate ferric phosphate slurry is subjected to solid-liquid separation, washed 1-5 times, and then sintered at 450-700° C. for 1-6 hours to obtain anhydrous ferric phosphate.
[0023] S9: The iron phosphate in step S8 is mixed with the lithium source and the coated carbon source, ground, dried and calcined to obtain a lithium iron phosphate material, which is used to evaluate the performance of the iron phosphate.
[0024] The iron source described in steps S1-S3 is at least one of ferroferric oxide, ferrous oxide, ferrous sulfate, ferrous chloride, ferrous nitrate, ferric sulfate, ferric chloride, and iron powder; the acid solution is at least one of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, and phosphoric acid solution; the impurity remover includes at least one of ammonia water, monoammonium dihydrogen phosphate, and iron powder; the impurity removal temperature is 20-90°C, further 40-60°C; the impurity removal time is 1-6h; the alkali solution is at least one of sodium hydroxide solution, calcium hydroxide, ammonia solution, sodium carbonate solution, and potassium hydroxide solution; the amount of alkali solution added is 0.5%-300% relative to the molar amount of iron; the oxidant is at least one of air, oxygen, ozone, and hydrogen peroxide; the amount added is 100%-200% relative to the molar amount of iron; the iron-active hydroxide intermediate is at least one of ferric hydroxide, basic ferric sulfate, basic ferric chloride, and basic ferric nitrate.
[0025] The number of pulping described in steps S4-S7 is 1 to 4 times; the phosphorus source is at least one of monoammonium phosphate, diammonium phosphate, triammonium phosphate, and phosphoric acid; the amount of water is 1 to 10 times the mass of the intermediate, and more preferably 3 to 8 times; the amount of B solution added is 98% to 105% of the molar amount of the iron source in the ferric phosphate intermediate active body; the insulation temperature is 70 to 99°C, and the insulation time is 0.2 to 2 hours, and more preferably 0.4 to 1 hour.
[0026] A device for preparing iron phosphate by precipitation conversion, as shown in the following Figure 6 As shown, including: Base 1; a stirring cylinder is arranged on the base 1; a heating resistor 10: arranged in the inner wall of the stirring cylinder, used to control the heating temperature of the liquid in the stirring cylinder; a lifting cylinder 2: a restraining end of the lifting cylinder 2 is fixed on the base 1, and a frame 4 is fixed to the end of a cylinder shaft 3 of the lifting cylinder 2 extending out of the cylinder; a motor 5: a restraining end of the motor 5 is fixed on the frame 4, and a rotating shaft 6 of the motor 5 extends into the interior of the stirring cylinder; Feeding plate 7: arranged at the opening above the mixing cylinder, the feeding plate 7 is coaxially fixed with the rotating shaft 6; feeding pipe 8: a plurality of leakage holes are evenly spaced in annular direction at the bottom of the feeding plate 7, each leakage hole is connected with a feeding pipe 8; the feeding pipe 8 is parallel to the rotating shaft 6; the rotating shaft 6 is fixedly connected with the feeding pipe 8 through a cross bar; stirring blade 9: the stirring blade 9 is connected with the feeding pipe 8; a nozzle is provided at the end of the stirring blade 9. The setting of the heating resistor 10 can stably maintain the temperature in the stirring tank and adjust it to the temperature required for the reaction; the rotating shaft 6 of the motor 5 is integrated with the feeding plate 7, the feeding pipe 8 and the stirring fan blade 9. At the end of the reaction, the cylinder is started by lifting the cylinder, and the cylinder shaft 3 moves upward, which can lift the rotating shaft 6 upward, so that there is no other structure in the stirring tank, which is convenient for subsequent processing of the liquid in the tank; this solution can realize the slow addition of reactants, avoiding the problem of poor reaction effect caused by excessive addition at one time. At the same time, adding materials according to the stirring rhythm can make the newly added raw materials fully contact with the reactants, thereby improving the reaction efficiency and saving reaction time.
[0027] Example 1 Step S1-3: Weigh a certain amount of ferroferric oxide, dissolve it in 20% HCl solution, obtain a FeClx mixed solution, obtain high-purity iron liquid by impurity removal process, and prepare it into a solution with an iron concentration of 1.5 mol / L. Take 200 ml of iron liquid in a reactor for stirring, add 0.165 mol of 30% hydrogen peroxide solution to oxidize for half an hour, then add 45 ml of 20% ammonia solution to the reactor, and react for 1 hour to obtain an iron active hydroxide intermediate; Steps S4-7: After solid-liquid separation of the iron active hydroxide intermediate in steps S1-3, pulping and washing are performed for 3 times, and the intermediate after pulping and filtration is dried for standby use; 0.2 mol of monoammonium phosphate and 0.112 mol of phosphoric acid solution are weighed to prepare 1.5 mol / L phosphorus liquid; then the dried and measured iron active hydroxide intermediate and phosphorus liquid are added to the reactor for stirring, and the temperature is raised to 97° C. for conversion reaction. After the temperature reaches 97° C., it is kept warm for 18 minutes to obtain dihydrate iron phosphate slurry; Step S8: solid-liquid separation of the dihydrate ferric phosphate slurry in steps S4 to S7, and slurry washing three times, drying the filter cake at 95° C. for 24 hours, and then sintering the dried filter cake at 500° C. for 4 hours to obtain an anhydrous ferric phosphate product; Step S9: Weigh a certain amount of iron phosphate, lithium carbonate (the molar ratio of iron:lithium is 1:1.03) and 11% starch relative to the mass of lithium iron phosphate, mix and grind them evenly and dry them, then sinter them at 700°C for 8h in an argon atmosphere to obtain lithium iron phosphate material.
[0028] Depend on Figure 1-Figure 5It can be seen that this scheme reduces the time for crystal transformation. The crystal transformation time for preparing iron phosphate by the traditional process is 1 to 2 hours. The transformation time of the present invention is very fast and can be completely transformed within 0.5 hours at 95°C. Lowering the transformation temperature will correspondingly extend the transformation time. Figure 1 It is indicated that the iron phosphate synthesized by the present invention has a porous nano-strip microstructure, which will have certain advantages in terms of product gram capacity and rate performance. Figure 2 It indicates that the iron phosphate synthesized by the present invention has a perfect crystal form without impurities after XRD diffraction pattern detection. Figure 3 It indicates that the iron phosphate synthesized by the present invention has excellent gram capacity and rate performance after button battery testing, with a 0.1C gram capacity of 160 mAh / g and a 1C gram capacity of 152 mAh / g, reaching or exceeding the performance of mainstream products in the industry. Figure 4 It indicates that the iron phosphate synthesized by the present invention has excellent cycle performance after button battery testing, and the capacity retention rate after 100 charge and discharge cycles is greater than 99%. Figure 5 It shows that the iron phosphate synthesized by the present invention has excellent fast charging performance after fast charging test of button batteries. At different fast charging rates of 1C-6C, the 1C discharge capacity is always greater than 152mAh / g. In summary, the finished products prepared by this scheme have improved performance.
[0029] Example 2 Step S1-3: Weigh a certain amount of titanium dioxide byproduct ferrous sulfate, dissolve it with water, obtain FeSO4 solution, use iron powder to carry out titanium reduction and impurity removal reaction, and prepare it into a solution with an iron concentration of 1.8 mol / L. Take 200 ml of iron liquid in a reactor and stir it, add 0.22 mol of 30% hydrogen peroxide solution to oxidize it for 45 minutes, and then add 42 ml of 30% sodium hydroxide solution to the reactor, and react for 1 hour to obtain an iron active hydroxide intermediate; Steps S4-7: After solid-liquid separation of the iron active hydroxide intermediate in steps S1-3, pulping and washing are performed for 2 times, and the intermediate after pulping and filtration is dried for standby use; 0.15 mol of monoammonium phosphate and 0.228 mol of phosphoric acid solution are weighed to prepare 1.5 mol / L phosphorus liquid; then the dried intermediate and phosphorus liquid are added to the reactor for stirring, and the temperature is raised to 95° C. for conversion reaction. After the temperature reaches 95° C., it is kept warm for 25 minutes to obtain dihydrate iron phosphate slurry; Step S8: solid-liquid separation of the dihydrate ferric phosphate slurry in steps S4 to S7, and slurry washing 4 times, drying the filter cake at 90° C. for 24 hours, and then sintering the dried filter cake at 520° C. for 4 hours to obtain an anhydrous ferric phosphate product; Step S9: Weigh a certain amount of iron phosphate, lithium carbonate (the molar ratio of iron:lithium is 1:1.03) and 11% of glucose relative to the mass of lithium iron phosphate, mix and grind them evenly and dry them, then sinter them at 700°C for 8h in an argon atmosphere to obtain lithium iron phosphate material.
[0030] Example 3 Step S1-3: Weigh a certain amount of ferrous chloride, dissolve it in water, and obtain a FeCl2 solution, which is configured to a solution with an iron concentration of 1.6 mol / L. Take 500 ml of molten iron in a reactor and stir it, add 0.6 mol of 30% hydrogen peroxide solution to it and oxidize it for 60 minutes, then add 156 ml of 20% ammonia solution to the reactor, and react for 1 hour to obtain an active iron hydroxide intermediate; Steps S4-7: After solid-liquid separation of the active iron hydroxide intermediate in steps S1-3, pulping and washing are performed for 4 times, and the intermediate after pulping and filtration is dried for standby use; 0.374 mol of diammonium phosphate and 0.45 mol of phosphoric acid solution are weighed to prepare 1.5 mol / L phosphorus liquid; then the dried intermediate and phosphorus liquid are added to the reactor for stirring, and the temperature is raised to 93° C. for conversion reaction. After the temperature reaches 93° C., it is kept warm for 40 minutes to obtain dihydrate iron phosphate slurry; Step S8: solid-liquid separation of the dihydrate ferric phosphate slurry in steps S4 to S7, and slurry washing three times, drying the filter cake at 105° C. for 24 hours, and then sintering the dried filter cake at 530° C. for 4 hours to obtain an anhydrous ferric phosphate product; Step S9: Weigh a certain amount of iron phosphate, lithium carbonate (the molar ratio of iron:lithium is 1:1.03) and 11% of citric acid monohydrate relative to the mass of lithium iron phosphate, mix and grind them evenly and dry them, then sinter them at 700°C for 8h in an argon atmosphere to obtain lithium iron phosphate material.
[0031] The above are only embodiments of the present invention. The invention is not limited to the fields involved in this implementation case. The common sense such as the known specific structures and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field to which the invention belongs before the application date or the priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to explain the content of the claims.
Claims
1. A method for preparing ferric phosphate by precipitation conversion, It is characterized in that The following steps are involved: S1: Dissolve the iron source in water or acid; S2: Add impurity remover, raise the temperature to 20-90°C, stir for 1-6 hours and then separate to obtain liquid A; S3: adding alkali solution to solution A to obtain an iron active hydroxide intermediate, wherein the amount of alkali solution added is 0.5% to 300% relative to the molar amount of iron; S4: pulping and washing the active iron hydroxide intermediate 1 to 4 times to obtain a filter cake; S5: dissolving the phosphorus source in water to obtain solution B; S6: drying and measuring the washed filter cake and adding it to the reactor, and adding 1 to 10 times the mass of water relative to the mass of the intermediate and 98% to 105% of the molar amount of the iron source in the iron active hydroxide intermediate to the reactor; S7: After stirring evenly, raise the temperature to 70-99°C and keep the temperature for 0.2-2h to obtain ferric phosphate dihydrate slurry; S8: The dihydrate ferric phosphate slurry is subjected to solid-liquid separation, washed 1-5 times, and then sintered at 450-700° C. for 1-6 hours to obtain anhydrous ferric phosphate.
2. The method for preparing ferric phosphate by precipitation conversion according to claim 1, Features: The iron source in step S1 is one or more of ferroferric oxide, ferrous oxide, ferrous sulfate, ferrous chloride, ferrous nitrate, ferric sulfate, ferric chloride, and iron powder.
3. The method for preparing ferric phosphate by precipitation conversion according to claim 2, Features: The iron source is ferric iron.
4. The method for preparing ferric phosphate by precipitation conversion according to claim 1, Features: The acid solution in step S1 includes one or more of sulfuric acid solution, hydrochloric acid solution, nitric acid solution, and phosphoric acid solution.
5. The method for preparing ferric phosphate by precipitation conversion according to claim 1, Features: The impurity remover in step S2 includes one or more of ammonia water, monoammonium dihydrogen phosphate, and iron powder.
6. The method for preparing ferric phosphate by precipitation conversion according to claim 1, Features: The alkali solution in step S3 is one or more of sodium hydroxide solution, calcium hydroxide, ammonia solution, sodium carbonate solution, and potassium hydroxide solution.
7. The method for preparing ferric phosphate by precipitation conversion according to claim 1, Features: The phosphorus source in step S5 is one or more of monoammonium phosphate, diammonium phosphate, triammonium phosphate, and phosphoric acid.
8. A device for preparing iron phosphate by precipitation conversion, It is characterized in that include: A base; a stirring cylinder is arranged on the base; Heating resistor: set in the inner wall of the mixing tank, used to control the heating temperature of the liquid in the mixing tank; Lifting cylinder: The restraining end of the lifting cylinder is fixed on the base, and the cylinder shaft end of the lifting cylinder extending out of the cylinder is fixed to the frame; Motor: The restraining end of the motor is fixed on the frame, and the rotating shaft of the motor extends into the mixing tank; Feeding plate: arranged at the opening above the mixing tank, the feeding plate is coaxially fixed with the rotating shaft; Feed pipe: a plurality of leakage holes are evenly spaced at the bottom of the feeding plate, each leakage hole is connected to a feed pipe; the feed pipe is parallel to the rotating shaft; the rotating shaft is fixedly connected to the feed pipe through a cross bar; Stirring blade: The stirring blade is connected with the material passing pipe; a nozzle is arranged at the end of the stirring blade.
Citation Information
Patent Citations
Preparation device, system and method of alkali cylinder for laboratory
CN112007538A
Iron phosphate dihydrate and preparation method thereof, iron phosphate, lithium iron phosphate and lithium ion battery
CN114394581A
Method for controllably preparing battery-grade iron phosphate from pyrite cinder
CN114906830A
Building materials thick liquids mixing stirring device
CN206701106U
Cited By
Low-compressive-collapse anhydrous iron phosphate material prepared by stress crystal transformation coupling and application of low-compressive-collapse anhydrous iron phosphate material
CN121020531A