Production process of lithium manganese iron phosphate

By adopting a mixing process of multiple iron phosphate and manganese sources, combined with sintering and crushing treatment, the shortcomings of lithium iron phosphate materials in electrical conductivity and cycling performance are solved, and higher compaction density and electrochemical performance are achieved, improving the The battery performance and safety are provided.

CN118929613AActive Publication Date: 2024-11-12ZIJIN MINING GROUP CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411198383.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Lithium manganese ferrophosphate materials have poor conductivity, rate performance and cyclic properties. When the electrochemical performance is improved by nano- nano-solution, the material will lack large particle support, the product compaction density will become lower and the energy density will be reduced.

Method used

Two different forms of iron phosphate are used as the iron source, combined with manganese dioxide and manganese carbonate, and the dosage ratio is optimized. Lithium manganese phosphate material with more uniform particle size is prepared through drying, spray drying and sintering processes, and combined with air flow crushing Treatment to form a product with regular morphology and high compaction density.

Benefits of technology

The compaction density and electrochemical performance of lithium manganese iron phosphate material are improved, the battery capacity and energy density are increased, the conductivity and cycling stability are improved, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929613A_ABST
    Figure CN118929613A_ABST
Patent Text Reader

Abstract

The invention discloses a production process of lithium manganese iron phosphate, and belongs to the technical field of electrode materials. Two different forms of iron phosphate are mixed as an iron source, manganese dioxide and manganese carbonate are matched at the same time, the dosage proportion is optimized, the lithium manganese iron phosphate material with more uniform particle size is prepared, and the obtained product is smaller in crystal particle size, more regular in particle morphology, higher in compaction density and higher in specific surface area. And the use performance and the safety of the prepared battery can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode materials, and in particular relates to a production process of lithium manganese iron phosphate. Background Art

[0002] Lithium manganese iron phosphate (LMFP) is considered in the industry to be an upgraded version of lithium iron phosphate. It has better thermal stability, chemical stability and economy than ternary materials, and at the same time has a higher energy density than lithium iron phosphate. However, lithium manganese iron phosphate also has problems such as poor conductivity, rate performance and cycle performance. At present, most companies on the market have improved the performance of lithium iron manganese phosphate through nano-processing to address the shortcomings of lithium iron manganese phosphate. Nano-processing reduces the crystal particle size of the material through mechanical ball milling, controlling the calcination temperature and other methods, thereby shortening the lithium ion diffusion path, improving the efficiency of lithium ion migration, and thus improving the rate performance of the material. While reducing the crystal particle size, the specific surface area of ​​the material is increased, thereby increasing the contact interface with the electrolyte, reducing the electrode interface impedance, and thus the electrochemical performance can be improved accordingly.

[0003] However, simply reducing the particle size of primary particles through nano-sizing to improve the electrochemical performance of the material will result in the material lacking support from large particles, lowering the compaction density of the product and reducing the energy density. Summary of the invention

[0004] In view of the problems raised in the background technology, the purpose of the present invention is to provide a production process of lithium manganese iron phosphate. The present invention adopts two different forms of iron phosphate mixed as the iron source, and at the same time cooperates with manganese dioxide and manganese carbonate, optimizes the dosage ratio, and prepares a lithium manganese iron phosphate material with more uniform particle size, high product uniformity and good overall performance.

[0005] The technical solution of the present invention is as follows: A production process of lithium manganese iron phosphate comprises the following steps: Step 1: Mix the flaky iron phosphate and the quasi-spherical iron phosphate as the iron source, and simultaneously take the lithium source, manganese source, carbon source and additives, and dry them separately for later use; Step 2: Add lithium source, manganese source, iron source, additives and carbon source to deionized water in sequence, stir and disperse continuously during the adding process, grind the obtained slurry, and then spray dry; Step 3: Sintering the spray-dried material obtained after spray drying under a protective gas atmosphere at 750-820° C., and crushing the material after sintering to obtain lithium manganese iron phosphate.

[0006] Furthermore, the lithium source in step 1 is lithium dihydrogen phosphate and lithium carbonate.

[0007] Furthermore, the manganese source in step 1 is composed of manganese dioxide and manganese carbonate, and the molar ratio of manganese elements in manganese dioxide and manganese carbonate is (0.5-2):1.

[0008] Furthermore, the carbon source in step 1 is PEG or glucose.

[0009] Furthermore, the additives in step one are magnesium oxide and titanium dioxide.

[0010] Furthermore, the drying in step 1 is carried out at 80-120° C. for 2-6 h.

[0011] Furthermore, in step 2, the addition amount of each raw material satisfies the manganese / iron molar ratio of 1 to 4, the (manganese + iron) / phosphorus molar ratio of 0.94 to 0.99, and the lithium / (manganese + iron) molar ratio of 1.01 to 1.08.

[0012] Furthermore, in step 2, the amount of carbon source added is 10%-15% of the total mass of the iron source and manganese source; the amount of additives added is 0.8%-1.5% of the total mass of the iron source and manganese source, among which the amount of magnesium oxide added is 0.5%-1.0% of the total mass of the iron source and manganese source, and the amount of titanium dioxide added is 0.3%-0.5% of the total mass of the iron source and manganese source.

[0013] Furthermore, in step 2, the solid content of the slurry is 30%-50%, the slurry is ground to a particle size D50 of 0.25-0.4 μm, and the pH is controlled to 6-9.

[0014] Furthermore, in step 2, the spray drying air inlet temperature is 190-220°C, and the air outlet temperature is 80-100°C.

[0015] Furthermore, the protective gas atmosphere in step three is at least one of a nitrogen atmosphere and an argon atmosphere.

[0016] Furthermore, in step three, the sintering heating rate is 1.5°C / min, and the holding time is 8-12 h.

[0017] Furthermore, in step 3, the pulverization after sintering is performed by air flow pulverization, and the pulverization particle size D50 is 0.5-2 μm.

[0018] Flake iron phosphate can form larger crystals at high temperatures, while spherical iron phosphate has smaller crystal particle size at the same temperature. The crystal particle size of lithium manganese iron phosphate material prepared by mixing the two iron phosphates tends to be of intermediate size, and the crystal morphology also tends to be regular, which can increase the compaction density of the material, improve the battery capacity and energy density, and improve the conductivity, ion transport and cycle stability of the battery material. When only one morphology of iron phosphate is used, since the crystal morphology of manganese dioxide and manganese carbonate can also achieve the above effect of iron phosphate at high temperature, by changing the ratio of manganese dioxide and manganese carbonate, the particle size of the prepared lithium manganese iron phosphate material is more uniform, the product uniformity is higher, and the overall performance is improved.

[0019] The process of the present invention adopts a mixed method of multiple iron phosphates and multiple manganese sources, and utilizes the different morphologies and reaction activities of different iron and manganese. During the sintering process, different nucleation and grain growth processes will occur. By preparing with a suitable ratio, lithium manganese iron phosphate with a large number of fine particles and a small amount of large particles can be obtained, thereby improving the compaction density and electrochemical performance.

[0020] The beneficial effects of the present invention are: 1. The preparation method of the present invention has a wide range of raw material sources and more selectivity for the main raw materials, and the preparation cost is low.

[0021] 2. The product obtained by the present invention has a smaller crystal particle size, a more regular particle morphology, and a higher compaction density, which can effectively improve the performance and safety of the prepared battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM image of the lithium manganese iron phosphate prepared in Example 1 of the present invention (magnification 20,000). DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0025] The raw materials for the experiment of the present invention are all commercially available, wherein the purity of the flake iron phosphate and the quasi-spherical iron phosphate are both 97%, the purity of manganese dioxide is 90%, the purity of manganese carbonate is 99.5%, the purity of lithium dihydrogen phosphate is 99.8%, and the purity of lithium carbonate is 99.8%.

[0026] Example 1 A production process of lithium iron manganese phosphate, comprising: 1. Weigh 1 kg of dried (80°C, 4 h) flaky iron phosphate, 1 kg of quasi-spherical iron phosphate, 0.567 kg of manganese dioxide, 1.587 kg of manganese carbonate, 2.078 kg of lithium dihydrogen phosphate, 0.516 kg of lithium carbonate, 0.03 kg of magnesium oxide, 0.015 kg of titanium dioxide, 0.3312 kg of PEG, 0.3888 kg of glucose, and 18.36 kg of deionized water for later use.

[0027] 2. Slowly add lithium carbonate (dispersed for 20 min), lithium dihydrogen phosphate (dissolved in water before adding, dispersed for 20 min), manganese carbonate, manganese dioxide, two kinds of iron phosphate (dispersed for 30 min), magnesium oxide, glucose, and PEG (dispersed for 40 min) to deionized water in sequence to obtain a slurry, which is then ground to control the slurry solid content to 40%, the particle size D50 = 0.32 μm, and the pH to 7.5.

[0028] 3. The obtained slurry is spray dried (inlet air temperature 210°C, outlet air temperature 90°C) to obtain a material with a moisture content of 1.2%; the spray dried material is transferred into a kiln for sintering (sintering temperature is 800°C, heating rate is 1.5°C / min, and insulation is 10 h). Nitrogen is introduced throughout the sintering process, and the oxygen content is controlled at 1-3 PPM; the sintered product is lithium manganese iron phosphate, which is crushed to D50=1-1.5 μm and packaged to obtain the finished product.

[0029] The SEM image of lithium manganese iron phosphate prepared in this example is as follows Figure 1 shown.

[0030] Referring to the step parameters of Example 1, Examples 2-7 and Comparative Examples 1-4 were designed, and the amounts of raw materials used are shown in Table 1 respectively.

[0031] The raw materials and dosages of the above examples and comparative examples are shown in the following table.

[0032] Table 1 Raw materials and dosage (unit: kg)

[0033] The performance of the lithium manganese iron phosphate samples prepared in the above examples and comparative examples was tested, and the results are as follows.

[0034] Table 2 Compacted density and electrochemical performance test results

[0035] In summary, the carbon source, additive addition amount and other preparation processes of Comparative Examples 1 to 4 are consistent with the embodiments, except that the ferromanganese source raw material adopts a single manganese source and a single iron phosphate. It can be seen from the data results in the table that the compaction density and electrochemical properties of the material can be improved by using different iron sources and different manganese sources together in the present invention. There are different grain nucleation and growth processes in the sintering process of different iron phosphates and different manganese sources selected by the present invention, and different ratios are adjusted at the same time, which can achieve a more excellent size particle grading effect, retain a large number of small particles while obtaining enough large particles, and effectively improve the compaction density and electrical properties.

[0036] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A production process of lithium manganese iron phosphate, characterized in that: The steps include: Step 1: Mix the flaky iron phosphate and the quasi-spherical iron phosphate as the iron source, and simultaneously take the lithium source, manganese source, carbon source and additives, and dry them separately for later use; Step 2: Add lithium source, manganese source, iron source, additives and carbon source to deionized water in sequence, stir and disperse continuously during the adding process, grind the obtained slurry, and then spray dry; Step 3: Sintering the spray-dried material obtained after spray drying under a protective gas atmosphere at 750-820° C., and crushing the material after sintering to obtain lithium manganese iron phosphate.

2. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: The lithium source in step 1 is lithium dihydrogen phosphate and lithium carbonate.

3. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: The manganese source in step 1 is composed of manganese dioxide and manganese carbonate, and the molar ratio of manganese elements in manganese dioxide and manganese carbonate is (0.5-2):

1.

4. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: The carbon source in step 1 is PEG or glucose.

5. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: The additives in step 1 are magnesium oxide and titanium dioxide.

6. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: In step 2, the addition amount of each raw material satisfies the manganese / iron molar ratio of 1 to 4, the (manganese + iron) / phosphorus molar ratio of 0.94 to 0.99, and the lithium / (manganese + iron) molar ratio of 1.01 to 1.

08.

7. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: In step 2, the amount of carbon source added is 10%-15% of the total mass of the iron source and manganese source; the amount of additives added is 0.8%-1.5% of the total mass of the iron source and manganese source, among which the amount of magnesium oxide added is 0.5%-1.0% of the total mass of the iron source and manganese source, and the amount of titanium dioxide added is 0.3%-0.5% of the total mass of the iron source and manganese source.

8. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: Step 2: Grind the slurry to a particle size of D50 of 0.25-0.4 μm and control the pH to 6-9.

9. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: In step 2, the spray drying air inlet temperature is 190-220°C, and the air outlet temperature is 80-100°C.

10. The production process of lithium iron manganese phosphate according to claim 1, characterized in that: The sintering heating rate in step 3 is 1.5°C / min, and the holding time is 8-12 h.

Citation Information

Patent Citations

  • Lithium iron phosphate positive electrode material and preparation method thereof and battery

    CN110048109A

  • Preparation method of high-energy-density lithium iron phosphate

    CN116835559A

  • Preparation method and application of lithium manganese iron phosphate material

    CN117658095A

  • Lithium ferric manganese phosphate composite material and preparation method thereof

    CN117712372A

  • Carbon-encapsulated lithium manganese iron phosphate material, and preparation method and use thereof