Method for separating lithium from iron lepidolite

Through the high-pressure and low-concentration acid combined with oxidation reaction lithium extraction method, the problems of high energy consumption and low recovery rate in lithium mica were solved, and efficient and environmentally friendly lithium recycling was achieved, suitable for industrial applications, simplifying the removal process and reducing the Waste liquid is generated.

CN118929706AActive Publication Date: 2024-11-12JIANGSU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411054937.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing methods of extracting lithium from lithium mica have problems such as high energy consumption, complex operation, large slag volume, difficulty in removing impurities, and low recovery rate. In particular, the energy consumption of roasting and press-cooking methods is high and the amount of slag produced is large. The acid leaching method cannot effectively prevent impurity ions from entering the leaching liquid, resulting in a low recovery rate of lithium.

Method used

The high-pressure and low-concentration acid combined with oxidation reaction is adopted to extract lithium. The impurity ions are precipitated through oxidation reaction, reducing the difficulty of removing impurities, improving the recovery rate of lithium, and obtaining high-purity lithium carbonate through calcium salt and carbonate solution treatment, simplifying the removal of impurities The process reduces the amount of acid and alkali and waste liquid generation.

Benefits of technology

It has achieved high recovery rate of lithium, simple operation, low energy consumption and low acid and alkali consumption. It is suitable for industrial batch lithium extraction, and has important social, economic and environmental value, and has promoted the sustainable development of the lithium battery field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929706A_ABST
    Figure CN118929706A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of extraction of lithium from lithium ore, and particularly discloses a method for separating lithium from iron lepidolite. The method for separating the lithium from the iron lepidolite comprises the following steps: mixing iron lepidolite powder and an acid solution, adding the mixture into a high-pressure reaction kettle, and carrying out an oxidation leaching reaction to obtain a lithium-containing leaching solution; adding calcium salt into the lithium-containing leachate until the pH value of the system is neutral or alkaline, and filtering to obtain filtrate; adding a carbonate solution into the filtrate to remove redundant calcium ions, filtering, concentrating the filtrate, adding a saturated carbonate solution into the concentrated solution, and carrying out precipitation reaction, filtering and drying to obtain the battery-grade lithium carbonate. According to the method for separating the lithium from the iron lepidolite, battery-grade lithium carbonate can be obtained, and the method is high in lithium recovery rate, simple to operate, low in energy consumption, low in acid and alkali consumption, small in waste liquid generation amount, suitable for industrial batch extraction of the lithium from the lithium ore, high in practical value and significant to sustainable development in the field of lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of extracting lithium from lithium ore, and in particular to a method for separating lithium from ferrolithium mica. Background Art

[0002] Lithium is considered to be an important strategic resource in this century. To a certain extent, it determines the lifeline of the development of the electric vehicle industry. It can be predicted that the global market demand for lithium will grow steadily for a long time in the future. Therefore, the development and utilization of lithium resources have received great attention and attention from all countries. There are three main types of lithium resources in nature: salt lakes (sulfates, carbonates, chlorides and nitrates, etc.), pegmatites (spodumene, lithium mica, etc.) and sedimentary rocks (bauxite, coal, kaolin, etc.). my country's lithium resources mainly exist in the form of salt lake lithium and lithium mica. Among them, salt lake lithium resources are relatively abundant, but there are problems such as high magnesium-lithium ratio in salt lakes, difficult separation and high cost. Although lithium mica resources are also relatively abundant, the grade of the mine is low, the cost of lithium extraction is high, and the environmental pollution is large.

[0003] The chemical formula of lithium iron mica is KLiFeAl(AlSi3O 10 )(F,OH)2, is a gray metallic layered silicate mineral belonging to the mica family, in which the Li2O content ranges from 1.1 to 5.0wt%. The methods for separating lithium from iron lithium mica mainly include dilute acid leaching, sulfate roasting, chlorination roasting, hydrofluoric acid method, pressure cooking, etc. However, the roasting method and pressure cooking method have high energy consumption, more reagents need to be added during the extraction process, and the amount of slag produced is large; the acid leaching method cannot avoid the entry of impurity ions into the leachate, and the impurity ions in the leachate need to be further removed. In the process of impurity removal, lithium loss will inevitably occur, resulting in a low lithium recovery rate. At the same time, the acid corrosiveness to the extraction equipment is relatively large. Therefore, it is urgent to develop a method for extracting lithium from lithium ore that is simple to operate, low in energy consumption, low in impurity removal difficulty and high in recovery rate. Summary of the invention

[0004] Aiming at the problems of high energy consumption, complex operation, large amount of slag, difficulty in impurity removal, low yield and difficulty in obtaining battery-grade lithium salt in the existing method for extracting lithium from lithium mica ore, the present invention provides a method for separating lithium from lithium iron mica, adopting a method for extracting lithium by combining high-pressure and low-concentration acid with oxidation reaction, without high-temperature roasting and high-concentration acid reaction, so that most of the leached impurity ions are precipitated in the form of ions, realizing lithium slag separation, reducing the difficulty of impurity removal, improving the recovery rate of lithium, reducing the amount of neutralizing reagent used, reducing the slag amount and corrosion to equipment, facilitating industrial application, and having important significance for promoting the sustainable development of lithium batteries.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0006] A method for separating lithium from iron lithium mica comprises the following steps:

[0007] Step a, crushing the iron lithium mica ore to obtain the iron lithium mica powder;

[0008] Step b, mixing the iron lithium mica powder and a low concentration acid solution uniformly to obtain a mixed material; the acid solution includes sulfuric acid;

[0009] Step c, subjecting the mixed material and the oxidant to an oxidation leaching reaction under high pressure conditions, and separating the solid from the liquid to obtain a lithium-containing leachate;

[0010] Step d, adding calcium salt to the lithium-containing leachate until the pH of the system is neutral or alkaline, and separating the solid and liquid to obtain a filtrate;

[0011] Step e, adding a carbonate solution to the filtrate to remove excess calcium ions, separating the solid and the liquid, and concentrating the obtained filtrate to obtain a concentrated solution;

[0012] Step f, adding a saturated carbonate solution to the concentrated solution, performing a precipitation reaction, solid-liquid separation, and drying to obtain battery-grade lithium carbonate.

[0013] The existing acid leaching method for lithium extraction requires the addition of alkaline substances to the lithium-containing acid leaching solution to remove iron ions and aluminum ions, and more Li will be entrained and precipitated during the precipitation process, especially when the precipitation amount is large, the entrained Li will be more. For example, the existing method generally adds calcium hydroxide or calcium carbonate to the lithium-containing acid solution to precipitate aluminum hydroxide. During the process, the lithium in the lithium-containing acid leaching solution and the aluminum hydroxide will generate a stable lithium sulfate-aluminum hydroxide complex salt compound. Furthermore, Fe will form iron oxyhydroxide in an alkaline environment, entraining a part of lithium, resulting in a large amount of lithium loss.

[0014] Compared with the prior art, the method for separating lithium from iron lithium mica provided by the present invention firstly leaches lithium under acidic conditions, and then removes Fe 2+ Oxidation is performed to make the oxidized Fe 3+ and Al 3+ The precipitates are in the form of alum and iron vanadium, and Si is precipitated in the form of silicon dioxide, which effectively reduces the leaching of Al and Fe impurity ions, not only reducing the large amount of precipitation produced in the subsequent alkali removal process, but also reducing the inclusion of Li in the precipitation, thereby effectively improving the recovery rate of Li; at the same time, since most of the Al and Fe impurities have been fixed and precipitated in the form of precipitation during the acid leaching of lithium, the impurity ion content in the lithium-containing extract is relatively low, and F only needs to be removed by simply adding calcium salt in the subsequent process. - , unprecipitated Al 3+ , Fe 3+ , and adding carbonate to remove excess Ca 2+A high-purity lithium-containing extract can be obtained, and finally battery-grade lithium carbonate can be obtained through a simple lithium precipitation reaction, which greatly simplifies the impurity removal process. In addition, when extracting lithium under high-pressure oxidation conditions, only a lower concentration of acid solution is needed to fully extract lithium from iron lithium mica, which not only reduces the amount of acid used, but also avoids the problem of introducing impurity salts in traditional high-temperature roasting methods.

[0015] By the method for separating lithium from iron lithium mica provided by the present invention, battery-grade lithium carbonate can be obtained, and the lithium recovery rate is high, the operation is simple, the energy consumption is low, the acid and alkali consumption is small, and the amount of waste liquid generated is small. It is suitable for industrial batch extraction of lithium from lithium ore, has high practical value, and is of great significance for the sustainable development of the lithium battery field.

[0016] Furthermore, in step a, the content of powder with a particle size of not less than 100 mesh in the iron lithium mica powder is ≥90%.

[0017] Furthermore, step a in the present invention specifically includes: drying, crushing, fine grinding and sieving the iron lithium mica ore to obtain iron lithium ore powder with a particle size of not less than 100 mesh and a powder quantity of ≥90%.

[0018] The preferred particle size of the iron-lithium ore powder is beneficial to promoting sufficient leaching and extraction of Li.

[0019] Furthermore, in step b, the concentration of the acid solution is 0.5 mol / L to 3 mol / L.

[0020] Furthermore, in step b, the acid solution is a sulfuric acid solution, or an acid solution mixed with at least one of hydrochloric acid and nitric acid.

[0021] Specifically, in step b, the acid solution is a sulfuric acid solution; or the acid solution is a mixed solution of sulfuric acid and hydrochloric acid; or the acid solution is a mixed solution of sulfuric acid and nitric acid.

[0022] Furthermore, in step b, the liquid-to-solid ratio of the acid solution to the iron lithium mica powder is (3-6) mL:1 g.

[0023] Oxidative leaching is carried out under high-pressure oxidation conditions, which effectively promotes the leaching of Li. The leaching and extraction of Li from lithium iron mica can be achieved by using an acid solution with a relatively low concentration. Compared with the traditional acid leaching method, the method provided by the present invention effectively reduces the amount and concentration of the acid solution, not only reduces the amount of subsequent alkali added, reduces the amount of waste residue and waste liquid generated, but also effectively reduces the corrosion to the equipment during the extraction process, and is more suitable for industrial applications.

[0024] Under the above acid solution concentration and addition ratio, the reaction in step c can be completed under the condition of pH < 1, so that Fe in the iron lithium mica is oxidized to form iron vanadium and Al is formed into alum.

[0025] Furthermore, in step c, the oxidant is at least one of oxygen, air, ozone, potassium persulfate, sodium persulfate or ammonium persulfate.

[0026] Preferably, in step c, the oxidant is oxygen.

[0027] Specifically, when the oxidant is oxygen, the main chemical reaction occurring in step c is:

[0028] 3K(AlFeLi)(Si3Al)O 10 (OH)F+3 / 4O2+15 / 2H2SO4+3 / 2H2O=2K(Al3(SO4)2(OH)6)↓+K(Fe3(SO4)2(OH)6)↓+3 / 2Li2SO4+9SiO2+3HF↑

[0029] Specifically, when the oxidant is persulfate, the main chemical reaction occurring in step c is:

[0030] 6K(AlFeLi)(Si3Al)O 10 (OH)F+3Me2S2O8+12H2SO4+6H2O=4K(Al3(SO4)2(OH)6)↓+2K(Fe3(SO4)2(OH)6)↓+3Li2SO4+18SiO2+6HF↑+3Me2SO4(Me=K + 、Na + NH4 + ).

[0031] During the oxidation leaching process, Fe in the iron lithium mica is oxidized to form iron vanadium, Al to form alum, and Si is precipitated in the form of silica sand (silicon dioxide), which effectively reduces the content of Fe and Al impurity ions in the lithium-containing leachate, and the iron vanadium and alum formed in the acidic solution will not be mixed with Li. At the same time, since most of the Fe and Al have been precipitated in this step, the amount of slag formed by the subsequent precipitation when the Fe, Al and F ions are removed is significantly reduced, thereby significantly reducing the entrainment of Li in the precipitate, effectively improving the recovery rate of Li, simplifying the lithium extraction step, and providing a new, efficient and environmentally friendly method for extracting lithium from iron lithium mica, which is of great significance for promoting the sustainable development of lithium batteries.

[0032] Furthermore, in step c, the molar ratio of the oxidant to Fe in the iron lithium mica powder is 0.5:1 to 1:1.

[0033] The present invention creatively utilizes the chemical components in ferrolithium mica to react with SO4 in sulfuric acid under oxidation conditions. 2-A chemical reaction is carried out to form iron vanadium and aluminum vanadium, so that the Fe and Al impurity ions are cleverly precipitated in the form of precipitation, effectively reducing the content of Fe and Al impurity ions in the lithium-containing leachate. In the process of lithium extraction, most of the Fe and Al impurities are removed at the same time, which effectively simplifies the subsequent impurity removal process and significantly reduces the amount of slag produced by the subsequent impurity removal, thereby reducing the entrainment loss of Li.

[0034] Furthermore, in step c, the temperature of the oxidation leaching reaction is 150° C. to 300° C., the pressure is 1 MPa to 6 MPa, and the time is 1 h to 10 h.

[0035] The leaching rate of lithium ions can be increased under the above high pressure leaching conditions.

[0036] Furthermore, in step d, the calcium salt is at least one of calcium oxide, calcium carbonate, calcium hydroxide, calcium chloride, calcium nitrate or calcium oxalate, or a mixed salt thereof with at least one of sodium hydroxide, potassium hydroxide, sodium carbonate or potassium carbonate.

[0037] Furthermore, in step d, the pH of the system is adjusted to 7-11.

[0038] Preferably, in step d, the pH of the system is adjusted to 8-9.

[0039] In the above preferred pH range, the removal rate of F, Al and Fe ions can be improved and the content of impurity ions in the extract can be reduced.

[0040] Furthermore, in step e, the carbonate solution is at least one of a sodium carbonate solution, a potassium carbonate solution, a sodium bicarbonate solution or a potassium bicarbonate solution.

[0041] Furthermore, in step e, the concentration of the carbonate solution is 150 g / L to 200 g / L.

[0042] Furthermore, in step e, the molar ratio of carbonate ions in the carbonate solution to calcium ions in the filtrate is 1:1 to 1.1:1.

[0043] Remove the excess Ca from step d 2+ Removal can improve the purity of the lithium-containing extract.

[0044] Furthermore, in step e, the concentration of lithium ions in the concentrated solution is 15 g / L to 25 g / L.

[0045] Furthermore, in step f, the saturated carbonate solution is at least one of a saturated sodium carbonate solution, a saturated potassium carbonate solution, a saturated sodium bicarbonate solution or a saturated potassium bicarbonate solution.

[0046] Furthermore, in step f, the molar ratio of carbonate ions in the saturated carbonate solution to lithium ions in the concentrated solution is 1:2 to 1.1:2.

[0047] Furthermore, in step f, the precipitation reaction temperature is 80° C. to 95° C., and the reaction time is 1 h to 2 h.

[0048] Compared with the prior art, the present invention has the following advantages:

[0049] (1) The present invention provides a novel method for extracting lithium from iron lithium mica. The method can fully leach and extract lithium from iron lithium mica by using a low-concentration sulfuric acid solution, effectively reducing the amount and concentration of acid, and reducing corrosion to equipment and the amount of waste liquid generated;

[0050] (2) The present invention performs leaching under oxidizing conditions, and can form Fe and Al precipitation during the leaching process, thereby reducing the leaching of Fe and Al impurity ions, achieving simultaneous lithium extraction and impurity removal, and at the same time, reducing the amount of precipitation generated during the alkali impurity removal process, reducing the entrainment loss of Li, and improving the recovery rate of Li;

[0051] (3) The present invention has the advantages of a short process flow, low acid and alkali consumption, and low waste liquid and waste residue generation. The reagents and raw materials used in the extraction process are cheap and easy to obtain, taking into account both environmental protection and economic benefits. It is a green, efficient and low-cost lithium extraction process that can be scaled up and is suitable for industrial batch extraction of lithium from iron lithium mica, and has important social, economic and environmental values. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0053] Figure 1 It is a schematic diagram of the process flow of extracting lithium from iron lithium mica ore in an embodiment of the present invention. DETAILED DESCRIPTION

[0054] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0055] Example 1

[0056] A method for separating lithium from iron lithium mica:

[0057] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.01%;

[0058] Step b, mixing the iron lithium mica powder and 3 mol / L sulfuric acid solution at a solid-liquid ratio of 1g:3mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the oxygen introduced to Fe in the iron lithium mica powder is 0.8:1, the reaction temperature is 250°C, the reaction pressure is 5MPa, the reaction time is 10h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 98.27%;

[0059] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 7.6, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.5 g / L;

[0060] Step d, adding 150 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%, and the loss rate of lithium is less than 1%;

[0061] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 16.97 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 90° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 92.03%, and the purity of the lithium carbonate is 99.66%.

[0062] Example 2

[0063] A method for separating lithium from iron lithium mica:

[0064] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.01%;

[0065] Step b, mixing the iron lithium mica powder and 2mol / L sulfuric acid solution in a solid-liquid ratio of 1g:3mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the introduced oxygen to Fe in the iron lithium mica powder is 0.8:1, the reaction temperature is 200°C, the reaction pressure is 5MPa, the reaction time is 2h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 95.25%;

[0066] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 8.1, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.45 g / L;

[0067] Step d, adding 150 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%, and the loss rate of lithium is less than 1%;

[0068] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 15.78 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 95° C. for 1 hour, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 92.24%, and the purity of the lithium carbonate is 99.61%.

[0069] Example 3

[0070] A method for separating lithium from iron lithium mica:

[0071] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.03%;

[0072] Step b, mixing the iron lithium mica powder and 3 mol / L sulfuric acid solution at a solid-liquid ratio of 1g:3mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the oxygen introduced to Fe in the iron lithium mica powder is 0.8:1, the reaction temperature is 150°C, the reaction pressure is 5MPa, the reaction time is 3h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 94.71%;

[0073] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 9.3, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.49 g / L;

[0074] Step d, adding 200 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.8%, and the loss rate of lithium is less than 1%;

[0075] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 20.25 g / L, adding a saturated sodium carbonate solution to the concentrated solution, wherein the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1:2, stirring and reacting at 80° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 90.81%, and the purity of the lithium carbonate is 99.53%.

[0076] Example 4

[0077] A method for separating lithium from iron lithium mica:

[0078] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.03%;

[0079] Step b, mixing the iron lithium mica powder and 0.5 mol / L sulfuric acid solution at a solid-liquid ratio of 1g:6mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the oxygen introduced to Fe in the iron lithium mica powder is 0.8:1, the reaction temperature is 300°C, the reaction pressure is 5MPa, the reaction time is 8h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 96.38%;

[0080] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 8.6, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.56 g / L;

[0081] Step d, adding 170 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%, and the loss rate of lithium is less than 1%;

[0082] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 24.14 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 85° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 91.21%, and the purity of the lithium carbonate is 99.58%.

[0083] Example 5

[0084] A method for separating lithium from iron lithium mica:

[0085] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 1.98%;

[0086] Step b, mixing the iron lithium mica powder and 1mol / L sulfuric acid solution in a solid-liquid ratio of 1g:4mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the oxygen introduced to Fe in the iron lithium mica powder is 0.8:1, the reaction temperature is 200°C, the reaction pressure is 1MPa, the reaction time is 3h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 97.18%;

[0087] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 9.3, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.55 g / L;

[0088] Step d, adding 200 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.8%, and the loss rate of lithium is less than 1%;

[0089] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 21.58 g / L, adding a saturated sodium carbonate solution to the concentrated solution, wherein the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1:2, stirring and reacting at 90° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 90.91%, and the purity of the lithium carbonate is 99.63%.

[0090] Example 6

[0091] A method for separating lithium from iron lithium mica:

[0092] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.01%;

[0093] Step b, mixing the iron lithium mica powder and 2mol / L sulfuric acid solution at a solid-liquid ratio of 1g:5mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the oxygen introduced to Fe in the iron lithium mica powder is 0.5:1, the reaction temperature is 250°C, the reaction pressure is 5MPa, the reaction time is 8h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 98.86%;

[0094] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 8.7, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.53 g / L;

[0095] Step d, adding 170 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%, and the loss rate of lithium is less than 1%;

[0096] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 18.25 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 85° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 91.12%, and the purity of the lithium carbonate is 99.58%.

[0097] Example 7

[0098] A method for separating lithium from iron lithium mica:

[0099] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.11%;

[0100] Step b, mixing the iron lithium mica powder and 2mol / L sulfuric acid solution in a solid-liquid ratio of 1g:5mL, adding the mixture into a high-pressure reactor for leaching reaction, introducing oxygen during the reaction, the molar ratio of the introduced oxygen to Fe in the iron lithium mica powder is 1:1, the reaction temperature is 200°C, the reaction pressure is 6MPa, the reaction time is 6h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are iron vanadium, aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 98.34%;

[0101] Step c, adding calcium oxide to the lithium-containing leachate A until the solution pH is 9.8, filtering to obtain a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride and calcium sulfate, and sampling and analysis are performed from the lithium-containing leachate C, wherein the content of calcium ions is 0.61 g / L;

[0102] Step d, adding 160 g / L sodium carbonate solution in an equimolar amount to the calcium ion to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%, and the loss rate of lithium is less than 1%;

[0103] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 17.69 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 90° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 92.31%, and the purity of the lithium carbonate is 99.72%.

[0104] Comparative Example 1

[0105] This comparative example provides a method for separating lithium from iron lithium mica. The only difference from Example 1 is that no oxidant is added during the leaching process, and the remaining steps are the same. The specific steps are as follows:

[0106] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.01%;

[0107] Step b, mixing the iron lithium mica powder and 3 mol / L sulfuric acid solution at a solid-liquid ratio of 1g:3mL, adding the mixture into a high-pressure reactor for leaching reaction, the reaction temperature being 250°C, the reaction pressure being 5MPa, the reaction time being 10h, and after the reaction is completed, filtering to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 97.02%;

[0108] Step c, adding calcium oxide to the lithium-containing leachate A until the pH value of the solution is 8.5, filtering, and obtaining a lithium-containing leachate C and a filter residue D; the physical phase of the filter residue D is mainly calcium fluoride, calcium sulfate, aluminum hydroxide and ferrous hydroxide. Sampling and analysis of the lithium-containing leachate C show that the lithium loss rate is 10.2%;

[0109] Step d, adding 150 g / L sodium carbonate solution in an equimolar amount to calcium ions to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%;

[0110] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 17.25 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 90° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 75.32%, and the purity of the lithium carbonate is 99.03%.

[0111] Comparative Example 2

[0112] This comparative example provides a method for separating lithium from iron lithium mica. The only difference from Example 1 is that no oxidant is added during the leaching process, but it is added simultaneously with calcium oxide in step c. The remaining steps are the same. The specific steps are as follows:

[0113] Step a, drying, crushing, and finely grinding the iron lithium mica ore, and passing it through a 100-mesh sieve to make the passing ratio reach more than 90%, to obtain the iron lithium mica powder, wherein the lithium oxide content is 2.01%;

[0114] Step b, mixing the iron lithium mica powder and 3 mol / L sulfuric acid solution at a solid-liquid ratio of 1g:3mL, adding the mixture into a high-pressure reactor for leaching reaction, the reaction temperature being 250°C, the reaction pressure being 5MPa, the reaction time being 10h, and filtering after the reaction to obtain a lithium-containing leachate A and a filter residue B; the main phases in the filter residue B are aluminum vanadium and silicon sand, and sampling and analysis are performed from the lithium-containing leachate A, and the leaching rate of Li is 96.85%;

[0115] Step c, adding calcium oxide to the lithium-containing leachate A until the pH value of the solution is 8.5, then adding hydrogen peroxide, the molar ratio of hydrogen peroxide to Fe in iron lithium mica is 0.8:1, filtering to obtain lithium-containing leachate C and filter residue D; the physical phase of the filter residue D is mainly calcium fluoride, calcium sulfate, aluminum hydroxide and ferric hydroxide, sampling and analysis from the lithium-containing leachate C, the lithium loss rate is 15.2%;

[0116] Step d, adding 150 g / L sodium carbonate solution in an equimolar amount to calcium ions to the lithium-containing leachate C, filtering, and obtaining a lithium-containing leachate E and a filter residue F; the physical phase of the filter residue F is mainly calcium carbonate, and sampling and analysis of the lithium-containing leachate E show that the removal rate of calcium ions is 99.9%;

[0117] Step e, concentrating the lithium-containing leaching solution E to obtain a concentrated solution with a lithium ion concentration of 17.36 g / L, adding a saturated sodium carbonate solution to the concentrated solution, the molar ratio of carbonate ions in the saturated sodium carbonate solution to lithium ions in the concentrated solution is 1.1:2, stirring and reacting at 90° C. for 2 hours, filtering while hot, washing with hot water at 100° C., and drying in an oven at 120° C. to obtain battery-grade lithium carbonate. The final measured lithium recovery rate is 80.34%, and the purity of the lithium carbonate is 98.23%.

[0118] In Examples 1 to 7, the oxidant may also be other oxidants defined in the present invention, such as air, ozone, persulfate, etc., and the acid solution obtained by acid leaching may also be a mixed acid solution of hydrochloric acid or nitric acid and sulfuric acid, as long as the amount added is within the limit of the present invention, the technical effects equivalent to those of the corresponding embodiments can be achieved. Similarly, carbonates or saturated carbonates, calcium salts, etc. may also be other substances defined in the present invention, as long as they are within the range defined in the present invention, the effects equivalent to those of the embodiments can be achieved.

[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for separating lithium from iron lithium mica, characterized in that: The following steps are involved: Step a, crushing the iron lithium mica ore to obtain the iron lithium mica powder; Step b, uniformly mixing the iron lithium mica powder with a low concentration acid solution to obtain a mixed material; wherein the acid solution includes a sulfuric acid solution; Step c, subjecting the mixed material and the oxidant to an oxidation leaching reaction under high pressure conditions, and separating the solid from the liquid to obtain a lithium-containing leachate; Step d, adding calcium salt to the lithium-containing leachate until the pH of the system is neutral or alkaline, and separating the solid and liquid to obtain a filtrate; Step e, adding a carbonate solution to the filtrate to remove excess calcium ions, separating the solid and the liquid, and concentrating the obtained filtrate to obtain a concentrated solution; Step f, adding a saturated carbonate solution to the concentrated solution, performing a precipitation reaction, solid-liquid separation, and drying to obtain battery-grade lithium carbonate.

2. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step a, the content of powder with a particle size not less than 100 mesh in the iron lithium mica powder is ≥90%.

3. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step b, the concentration of the acid solution is 0.5 mol / L to 3 mol / L.

4. The method for separating lithium from iron lithium mica according to claim 1 or 3, characterized in that: In step b, the acid solution is a sulfuric acid solution, or a mixture of sulfuric acid and at least one of hydrochloric acid and nitric acid; and / or In step b, the liquid-to-solid ratio of the acid solution to the iron lithium mica powder is (3-6) mL:1 g.

5. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step c, the oxidant is at least one of oxygen, air, ozone, potassium persulfate, sodium persulfate or ammonium persulfate.

6. The method for separating lithium from iron lithium mica according to claim 1 or 5, characterized in that: In step c, the molar ratio of the oxidant to Fe in the iron lithium mica powder is 0.5:1 to 1:

1.

7. The method for separating lithium from iron lithium mica according to claim 1 or 5, characterized in that: In step c, the temperature of the oxidation leaching reaction is 150° C. to 300° C., the pressure is 1 MPa to 6 MPa, and the time is 1 h to 10 h.

8. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step d, the calcium salt is at least one of calcium oxide, calcium carbonate, calcium hydroxide, calcium chloride, calcium nitrate or calcium oxalate, or a mixed salt thereof with at least one of sodium hydroxide, potassium hydroxide, sodium carbonate or potassium carbonate; and / or In step d, the pH of the system is adjusted to 7-11.

9. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step e, the carbonate solution is at least one of a sodium carbonate solution, a potassium carbonate solution, a sodium bicarbonate solution or a potassium bicarbonate solution; and / or In step e, the molar ratio of carbonate ions in the carbonate solution to calcium ions in the filtrate is 1:1 to 1.1:1; and / or In step e, the concentration of lithium ions in the concentrated solution is 15 g / L to 25 g / L.

10. The method for separating lithium from iron lithium mica according to claim 1, characterized in that: In step f, the saturated carbonate solution is at least one of a saturated sodium carbonate solution, a saturated potassium carbonate solution, a saturated sodium bicarbonate solution or a saturated potassium bicarbonate solution; and / or In step f, the molar ratio of carbonate ions in the saturated carbonate solution to lithium ions in the concentrated solution is 1:2 to 1.1:2; and / or In step f, the precipitation reaction temperature is 80° C. to 95° C., and the reaction time is 1 h to 2 h.

Citation Information

Patent Citations

  • Method for producing refined lithium sulfate solution used in lepidolite lithium-extracting technique by sulfuric acid process

    CN101186968A

  • Method for acquiring lithium carbonate in zinnwaldite

    CN104649302A

  • Method for preparing lithium carbonate and potassium sulfate by using zinnwaldite

    CN105152188A

  • Method of extracting lithium carbonate from lepidolite ore

    CN107098365A

  • Method for preparing battery-grade lithium carbonate by taking lepidolite as raw material

    CN112645363A