Method for preparing vanadium pentoxide from high-chromium vanadium slag

By employing processes such as magnetic separation for iron removal, air separation for impurity removal, roasting, and wet grinding on high-chromium vanadium slag, and optimizing the rotary kiln speed and refractory material lining, the problem of low vanadium conversion rate in high-chromium vanadium slag has been solved, achieving efficient vanadium recovery and cost reduction.

CN118929751APending Publication Date: 2024-11-12CHENGDE YANBEI METALLURGY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411003129.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

How to achieve efficient and clean extraction and separation of vanadium and chromium from high-chromium vanadium slag, improve vanadium recovery rate, and reduce the cost and pollution problems of the vanadium extraction industry.

Method used

After crushing high-chromium vanadium slag, magnetic separation is used to remove iron, followed by grinding and air classification to remove impurities. The slag is then mixed with sodium salts and roasted. By combining wet grinding and post-treatment processes, the rotation speed of the rotary kiln and the refractory material lining are optimized to improve the conversion and recovery rate of vanadium.

Benefits of technology

It improves vanadium recovery rate, reduces costs, solves the problem of low vanadium conversion rate in high-chromium vanadium slag, and has a simple process with good prospects for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929751A_ABST
    Figure CN118929751A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing vanadium pentoxide by using high-chromium vanadium slag. The method comprises the following steps: (1) after crushing the high-chromium vanadium slag, sequentially carrying out magnetic separation iron removal, grinding treatment and winnowing impurity removal to obtain refined vanadium slag; (2) sodium salt and the refined vanadium slag obtained in the step (1) are mixed and then roasted in a rotary kiln, and clinker is obtained; and (3) carrying out wet grinding on the clinker obtained in the step (2), and carrying out post-treatment to obtain the vanadium pentoxide. The method provided by the invention can effectively solve the problem that the conversion rate of clinker vanadium is low after the chromium content in the vanadium slag is increased; according to the method, the recovery rate of vanadium is effectively increased, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium chemical industry, and particularly relates to a method for preparing vanadium pentoxide by utilizing high-chromium vanadium slag. Background Art

[0002] As an important industrial raw material, vanadium has a wide range of uses, including: as an alloying element or alloy additive, about 90% of vanadium is used in the steel industry; as the main active ingredient in the sulfuric acid industry and industrial denitrification catalysts; in the form of vanadium-containing alloys, it is used in the nuclear industry and aerospace; because of its colorful colors, it can be used as a pigment in the production of ceramic coloring, colored glass and ink; as an electrode material or electrolyte in the energy industry; as an effective trace component of medicine in the medical field. In particular, the industrial application status of high-purity vanadium pentoxide is getting higher and higher. As a raw material for the preparation of high-end products, high-purity vanadium pentoxide can be used in many high-tech industries: energy field, such as vanadium oxide lithium batteries, all-vanadium liquid flow batteries; the preparation of vanadium aluminum alloys is used in aerospace, military and civilian use; preparation of industrial catalysts: preparation of luminescent materials.

[0003] At present, the vanadium pentoxide slag produced includes high chromium vanadium slag, and its Cr2O3 content is between 8% and 12%. High chromium vanadium slag is a by-product of the smelting process of high chromium vanadium-titanium magnetite. Both vanadium and chromium have relatively high grades, so it is a potential raw material for vanadium and chromium extraction. Cr2O3 is a component that forms the spinel nucleus of vanadium slag, which is all concentrated in the spinel phase. The molten iron with more chromium can produce a large number of nuclei during the vanadium blowing process, which increases the viscosity of the initial slag. If the vanadium blowing temperature is not properly controlled, the generated vanadium slag will contain a large number of fine spinels, which is not conducive to the extraction of vanadium and the vanadium recovery rate is low.

[0004] Therefore, how to achieve efficient and clean extraction and separation of vanadium and chromium from high-chromium vanadium slag is an urgent problem to be solved in the vanadium chemical industry.

[0005] In addition, in the traditional vanadium slag vanadium extraction process, ammonium salts need to be further added to the vanadium-containing leaching solution to precipitate the vanadium in the form of ammonium vanadate. In this process, a large amount of ammonia nitrogen wastewater will be generated, which will cause great water pollution. The cost loss caused by the treatment of ammonia nitrogen wastewater is inevitable in the vanadium chemical industry. How to reduce the cost of the vanadium extraction industry and solve the pollution problem also needs to be considered. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing vanadium pentoxide using high-chromium vanadium slag. The method solves the problem of low clinker vanadium conversion rate caused by increased chromium content in vanadium slag, improves vanadium recovery rate and reduces cost.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for preparing vanadium pentoxide by using high-chromium vanadium slag, the method comprising the following steps:

[0009] (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron, grinding, and air separation to remove impurities, to obtain refined vanadium slag;

[0010] (2) mixing the sodium salt and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln to obtain clinker;

[0011] (3) The clinker obtained in step (2) is wet-grinded and post-treated to obtain the vanadium pentoxide.

[0012] The present invention improves the fineness of the refined vanadium slag and reduces its iron content by removing iron, air separation and grinding the high-chrome vanadium slag, so that the central part of the spinel in the high-chrome vanadium slag is fully exposed, and the solubility conversion of part of V2O3 in the crystal is realized; then the conversion rate of clinker vanadium is improved by sodium roasting; and finally, vanadium pentoxide is extracted by post-treatment. The method of the present invention solves the problem of low clinker vanadium conversion rate caused by increased chromium content in vanadium slag, improves the recovery rate of vanadium and reduces costs.

[0013] As a preferred technical solution of the present invention, the chromium content in the high chromium vanadium slag in step (1) is 8-12wt% as Cr2O3, the vanadium content is 12-15wt% as V2O5, and the iron content is 15-18wt% as elemental iron.

[0014] Exemplarily, the chromium content in the high chromium vanadium slag is 8 to 12 wt% in terms of Cr2O3, for example, 8 wt%, 9 wt%, 10 wt%, 11 wt% or 12 wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] The vanadium content in the high chromium vanadium slag is 12 to 15wt% in terms of V2O5, for example, it can be 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt%, 14.5wt% or 15wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] The iron content in the high chromium-vanadium slag is 15-18wt% in terms of elemental iron, for example, it can be 15wt%, 15.5wt%, 16wt%, 16.5wt%, 17wt%, 17.5wt% or 18wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] Preferably, the magnetic field strength of the magnetic separation and iron removal in step (1) is 50-70mT, for example, it can be 50mT, 55mT, 60mT, 65mT or 70mT, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, the grinding process in step (1) comprises coarse ball milling and fine ball milling performed sequentially.

[0019] Preferably, the rotation speed of the grinding treatment in step (1) is 20 to 22 r / min, for example, it can be 20 r / min, 20.5 r / min, 21 r / min, 21.5 r / min or 22 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] Preferably, the diameter of the grinding balls used in the coarse ball milling is 60-100 mm, for example, 60 mm, 70 mm, 80 mm, 90 mm or 100 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0021] Preferably, the diameter of the grinding balls used in the fine ball mill is 30-60 mm, for example, 30 mm, 40 mm, 50 mm or 60 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] Preferably, the grinding balls are high chromium alloy steel balls.

[0023] Preferably, the pressure of the air separation and impurity removal in step (1) is 2.5-3.5 kPa, for example, it can be 2.5 kPa, 2.7 kPa, 2.9 kPa, 3.1 kPa, 3.3 kPa or 3.5 kPa, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] In the present invention, the pressure of the air separation and impurity removal is 2.5-3.5 kPa. If the pressure is too low, it will lead to insufficient circulating air volume and the product fineness will not meet the requirements. If the pressure is too high, it will lead to excessive air volume, too fine product fineness and reduced work efficiency.

[0025] Preferably, the iron content in the refined vanadium slag in step (1) is 1.5-3wt%, for example, it can be 1.5wt%, 1.8wt%, 2.1wt%, 2.4wt%, 2.7wt% or 3wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] In the present invention, the iron content in the refined vanadium slag is 1.5-3wt%. If the iron content is too high, it will cause overheating, ring formation, and decreased conversion rate at the kiln tail, and at the same time, some oxidized vanadium will be reduced to low-valent vanadium.

[0027] Preferably, the particle size range of the refined vanadium slag in step (1) is 100-150 mesh, for example, it can be 100 mesh, 110 mesh, 120 mesh, 130 mesh, 140 mesh or 150 mesh, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] As a preferred technical solution of the present invention, the sodium salt in step (2) includes sodium carbonate and sodium chloride.

[0029] Preferably, the addition amount of sodium carbonate is 70-80% of the mass of the refined vanadium slag, for example, it can be 70%, 72%, 74%, 76%, 78% or 80%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the amount of sodium chloride added is 20-30% of the mass of the refined vanadium slag, for example, it can be 20%, 22%, 24%, 26%, 28% or 30%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] As a preferred technical solution of the present invention, the rotation speed of the rotary kiln is 0.3-0.68 r / min, for example, it can be 0.3 r / min, 0.4 r / min, 0.5 r / min, 0.6 r / min or 0.68 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] More specifically, when the specification of the rotary kiln is When the feed rate is 6.9 tons / hour, the rotation speed of the rotary kiln is 0.66-0.68 r / min, for example, it can be 0.66 r / min, 0.664 r / min, 0.668 r / min, 0.672 r / min, 0.676 r / min or 0.68 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] When the specification of the rotary kiln is When the feed rate is 16 tons / hour, the rotation speed of the rotary kiln is 0.3-0.33 r / min, for example, it can be 0.3 r / min, 0.305 r / min, 0.31 r / min, 0.315 r / min, 0.32 r / min, 0.325 r / min or 0.33 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] In the present invention, the rotation speed of the rotary kiln is reduced, the residence time of the material in the rotary kiln is prolonged, the oxidation and sodiumization time of the trivalent vanadium ions is increased, and thus the conversion rate of vanadium pentoxide is increased.

[0035] Preferably, refractory materials are laid at intervals on the inner wall of the rotary kiln.

[0036] Preferably, castables are laid between adjacent refractory materials.

[0037] In the present invention, the refractory material and the castable material are laid alternately on the same plane.

[0038] Preferably, the spacing between adjacent refractory materials is 180-220 mm, for example, 180 mm, 190 mm, 200 mm, 210 mm or 220 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the laying height difference between the refractory material and the castable is 10-15 mm, for example, it can be 10 mm, 11 mm, 12 mm, 13 mm, 14 mm or 15 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] The present invention further optimizes the masonry method of the refractory material inside the rotary kiln. By alternately arranging the refractory material and the castable and providing a height difference of 10 to 15 mm, the interior of the rotary kiln has the function of a lifting plate, which is beneficial to achieving full contact between the material and oxygen and improving the oxidation rate of vanadium.

[0041] As a preferred technical solution of the present invention, the time for the calcination treatment in step (2) is 260 to 300 minutes, for example, it can be 260 minutes, 270 minutes, 280 minutes, 290 minutes or 300 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] The present invention prolongs the roasting treatment time by reducing the rotation speed of the rotary kiln. More specifically, the extended time is the time of oxidative roasting, which is more conducive to the full oxidation of trivalent vanadium ions, creates conditions for sodiumization, and improves the conversion rate of vanadium.

[0043] Preferably, the roasting treatment in step (2) includes oxidation roasting, sodium roasting and cooling treatment performed in sequence.

[0044] Preferably, the terminal temperature of the oxidative roasting is 600-700°C, for example, 600°C, 620°C, 640°C, 660°C, 680°C or 700°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] Preferably, the endpoint temperature of the sodium roasting is 800-850°C, for example, 800°C, 810°C, 820°C, 830°C, 840°C or 850°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] In the present invention, the terminal temperature of the sodium roasting is 800-850°C. If the temperature is too high, impurities such as calcium, aluminum, and chromium will react, affecting the conversion rate of vanadium. It will also cause ring formation in the kiln, affecting ventilation and material reaction. If the temperature is too low, the vanadium iron spinel cannot be fully decomposed and oxidized, resulting in a low conversion rate of vanadium.

[0047] Preferably, the terminal temperature of the cooling treatment is 550-600°C, for example, it can be 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0048] As a preferred technical solution of the present invention, the solid-to-liquid ratio of clinker to water in the wet grinding of step (3) is 1:2.5-3.5, for example, it can be 1:2.5, 1:2.7, 1:2.9, 1:3.1, 1:3.3 or 1:3.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0049] Preferably, the wet grinding time in step (3) is 3 to 5 min, for example, 3 min, 3.4 min, 3.8 min, 4.2 min, 4.6 min or 5 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the wet grinding in step (3) also includes a cooling process after exiting the furnace.

[0051] As a preferred technical solution of the present invention, the post-treatment in step (3) comprises: sequentially performing leaching filtration and vanadium precipitation treatment to obtain ammonium polyvanadate, and then sequentially performing drying treatment, calcination deammoniation and melting treatment to obtain the vanadium pentoxide.

[0052] As a preferred technical solution of the present invention, the vanadium precipitation treatment comprises: mixing calcium chloride and the filtrate obtained by leaching and filtration to remove phosphorus, obtaining a supernatant after standing, and then mixing the supernatant, sulfuric acid and ammonium salt to vanadium precipitation treatment;

[0053] Preferably, the amount of calcium chloride added is 0.014-0.018wt% of the mass of the filtrate, for example, it can be 0.014wt%, 0.015wt%, 0.016wt%, 0.017wt% or 0.018wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0054] Preferably, the standing time is 12 to 24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0055] In the vanadium precipitation process of the present invention, the reaction liquid in the reaction system is in a boiling state, thereby realizing the formation of ammonium polyvanadate complex; further, in the vanadium precipitation process, sulfuric acid and the supernatant are first mixed until the pH value of the system is 1.7-2.5, and then ammonium sulfate is mixed; the ammonium sulfate addition coefficient is 0.95-1.25, for example, it can be 0.95, 1, 1.05, 1.1, 1.15, 1.2 or 1.25, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] Preferably, the water content of the ammonium polyvanadate is 35-45wt%, for example, 35wt%, 37wt%, 39wt%, 41wt%, 43wt% or 45wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0057] As a preferred technical solution of the present invention, the temperature of the drying treatment is 300-350°C, for example, it can be 300°C, 310°C, 320°C, 330°C, 340°C or 350°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0058] Preferably, the temperature of the calcination deamination is 400-600°C, for example, 400°C, 440°C, 480°C, 520°C, 560°C or 600°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0059] Preferably, the temperature of the melting treatment is 820-1050°C, for example, it can be 820°C, 860°C, 900°C, 940°C, 980°C, 1020°C or 1050°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0060] As a preferred technical solution of the present invention, the method for preparing vanadium pentoxide using high chromium vanadium slag provided by the present invention comprises the following steps:

[0061] (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron at a magnetic field strength of 50 to 70 mT, and then performing coarse ball milling and fine ball milling, and then performing air separation to remove impurities at a pressure of 2.5 to 3.5 kPa to obtain refined vanadium slag with an iron content of 1.5 to 3 wt% and a particle size range of 100 to 150 mesh;

[0062] The high chromium-vanadium slag has a chromium content of 8-12 wt% in terms of Cr2O3, a vanadium content of 12-15 wt% in terms of V2O5, and an iron content of 15-18 wt% in terms of elemental iron;

[0063] (2) mixing sodium carbonate, sodium chloride and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln for 260 to 300 minutes and then cooling the mixture to obtain clinker;

[0064] The amount of sodium carbonate added is 70-80% of the mass of the refined vanadium slag, and the amount of sodium chloride added is 20-30% of the mass of the refined vanadium slag;

[0065] The rotation speed of the rotary kiln is 0.3-0.68 r / min. Refractory materials are laid on the inner wall of the rotary kiln at intervals, and castables are laid between adjacent refractory materials; the spacing between adjacent refractory materials is 180-220 mm; the laying height difference between the refractory materials and the castables is 10-15 mm;

[0066] The roasting treatment includes oxidation roasting, sodium roasting and cooling treatment performed in sequence; the end temperature of the oxidation roasting is 600-700°C, the end temperature of the sodium roasting is 800-850°C, and the end temperature of the cooling treatment is 550-600°C;

[0067] (3) mixing clinker and water at a solid-liquid ratio of 1:2.5-3.5 for wet grinding for 3-5 minutes, leaching and filtering, mixing calcium chloride and the filtrate obtained by leaching and filtering for phosphorus removal, standing for 12-24 hours to obtain a supernatant, and then mixing the supernatant, sulfuric acid and ammonium salt for vanadium precipitation treatment to obtain ammonium polyvanadate with a water content of 35-45wt%;

[0068] The ammonium polyvanadate is dried at 300-350°C, then calcined at 400-500°C for deammoniation, and melted at 820-1050°C to obtain the vanadium pentoxide.

[0069] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0070] Compared with the prior art, the present invention has the following beneficial effects:

[0071] (1) The present invention optimizes the iron removal process of high-chrome vanadium slag, controls the iron content of refined vanadium slag to ≤3.0%, improves the fineness of refined vanadium slag, makes the central part of spinel in vanadium slag fully exposed, and realizes the soluble conversion of part of V2O3 in crystal;

[0072] (2) The present invention prolongs the residence time of the material in the rotary kiln by reducing the rotation speed of the rotary kiln, thereby improving V 3+ The oxidation and sodiumization time of the ions can improve the vanadium conversion rate and the recovery rate;

[0073] (3) The present invention changes the masonry form of the refractory material in the rotary kiln so that it plays the role of a lifting plate, thereby achieving full contact between the material and oxygen and improving the oxidation rate of vanadium;

[0074] (4) The method provided by the present invention couples the impurity and iron removal process, the sodium roasting process and the clinker post-treatment process, which effectively solves the problem of low vanadium recovery rate in high-chromium vanadium slag. The method has a simple process and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 This is a flow chart of a method for preparing vanadium pentoxide using high chromium vanadium slag provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0076] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0077] Example 1

[0078] This embodiment provides a Figure 1 The method for preparing vanadium pentoxide using high chromium vanadium slag comprises the following steps:

[0079] (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron at a magnetic field strength of 60 mT, and then performing coarse ball milling and fine ball milling, and then performing air separation to remove impurities at a pressure of 3 kPa to obtain refined vanadium slag with an iron content of 2.5 wt% and a particle size range of 120 to 150 mesh;

[0080] The high chromium-vanadium slag has a chromium content of 10 wt% calculated as Cr2O3, a vanadium content of 13.5 wt% calculated as V2O5, and an iron content of 16.5 wt% calculated as elemental iron;

[0081] (2) mixing sodium carbonate, sodium chloride and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln for 280 minutes and then cooling the mixture to obtain clinker;

[0082] The amount of sodium carbonate added is 75% of the mass of the refined vanadium slag, and the amount of sodium chloride added is 25% of the mass of the refined vanadium slag;

[0083] The rotation speed of the rotary kiln is 0.67r / min. Refractory materials are laid on the inner wall of the rotary kiln at intervals, and castables are laid between adjacent refractory materials; the spacing between adjacent refractory materials is 200mm; the laying height difference between the refractory materials and the castables is 10mm;

[0084] The roasting treatment includes oxidation roasting, sodium roasting and cooling treatment performed in sequence; the end temperature of the oxidation roasting is 650°C, the end temperature of the sodium roasting is 825°C, and the end temperature of the cooling treatment is 575°C;

[0085] (3) mixing clinker and water at a solid-liquid ratio of 1:3 and wet grinding for 4 minutes, leaching and filtering, mixing calcium chloride and the filtrate obtained by leaching and filtering for phosphorus removal, standing for 16 hours to obtain a supernatant, and then adding sulfuric acid at 100° C. and adjusting the pH value to 2, and then adding ammonium sulfate for vanadium precipitation to obtain ammonium polyvanadate with a water content of 40wt%; the ammonium sulfate addition coefficient is 1.1;

[0086] The ammonium polyvanadate is dried at 325°C, then calcined at 450°C for deammoniation, and melted at 950°C to obtain the vanadium pentoxide.

[0087] Example 2

[0088] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, the method comprising the following steps:

[0089] (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron at a magnetic field strength of 50 mT, and then performing coarse ball milling and fine ball milling, and then performing air separation to remove impurities at a pressure of 2.5 kPa to obtain refined vanadium slag with an iron content of 1.5 wt% and a particle size range of 130 to 150 mesh;

[0090] The high chromium-vanadium slag has a chromium content of 8wt% calculated as Cr2O3, a vanadium content of 12wt% calculated as V2O5, and an iron content of 15wt% calculated as elemental iron;

[0091] (2) mixing sodium carbonate, sodium chloride and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln for 260 minutes and then cooling the mixture to obtain clinker;

[0092] The amount of sodium carbonate added is 70% of the mass of the refined vanadium slag, and the amount of sodium chloride added is 30% of the mass of the refined vanadium slag;

[0093] The rotation speed of the rotary kiln is 0.68r / min. Refractory materials are laid on the inner wall of the rotary kiln at intervals, and castables are laid between adjacent refractory materials; the spacing between adjacent refractory materials is 180mm; the laying height difference between the refractory materials and the castables is 12.5mm;

[0094] The roasting treatment includes oxidation roasting, sodium roasting and cooling treatment performed in sequence; the end temperature of the oxidation roasting is 600°C, the end temperature of the sodium roasting is 800°C, and the end temperature of the cooling treatment is 550°C;

[0095] (3) mixing clinker and water at a solid-liquid ratio of 1:2.5 for wet grinding for 3 minutes, leaching and filtering, mixing calcium chloride and the filtrate obtained by leaching and filtering for phosphorus removal, standing for 12 hours to obtain a supernatant, and then mixing sulfuric acid and the supernatant at 100° C. until the pH value of the system is 1.7, and then mixing with ammonium sulfate for leaching and vanadium precipitation to obtain ammonium polyvanadate with a water content of 35wt%; the ammonium sulfate addition coefficient is 0.95;

[0096] The ammonium polyvanadate is dried at 300°C, then calcined at 400°C for deammoniation, and melted at 820°C to obtain the vanadium pentoxide.

[0097] Example 3

[0098] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, the method comprising the following steps:

[0099] (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron at a magnetic field strength of 70 mT, and then performing coarse ball milling and fine ball milling, and then performing air separation to remove impurities at a pressure of 3.5 kPa to obtain refined vanadium slag with an iron content of 3 wt% and a particle size range of 100 to 120 meshes;

[0100] The high chromium-vanadium slag has a chromium content of 12 wt% calculated as Cr2O3, a vanadium content of 15 wt% calculated as V2O5, and an iron content of 18 wt% calculated as elemental iron;

[0101] (2) mixing sodium carbonate, sodium chloride and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln for 300 minutes and then cooling the mixture to obtain clinker;

[0102] The amount of sodium carbonate added is 80% of the mass of the refined vanadium slag, and the amount of sodium chloride added is 20% of the mass of the refined vanadium slag;

[0103] The rotation speed of the rotary kiln is 0.32r / min. Refractory materials are laid on the inner wall of the rotary kiln at intervals, and castables are laid between adjacent refractory materials; the spacing between adjacent refractory materials is 220mm; the laying height difference between the refractory materials and the castables is 15mm;

[0104] The roasting treatment includes oxidation roasting, sodium roasting and cooling treatment performed in sequence; the end temperature of the oxidation roasting is 700°C, the end temperature of the sodium roasting is 850°C, and the end temperature of the cooling treatment is 600°C;

[0105] (3) mixing clinker and water at a solid-liquid ratio of 1:3.5 for wet grinding for 5 minutes, leaching and filtering, mixing calcium chloride and the filtrate obtained by leaching and filtering for phosphorus removal, standing for 24 hours to obtain a supernatant, and then mixing sulfuric acid and the supernatant at 100° C. until the pH value of the system is 2.5, and then mixing with ammonium sulfate for leaching and vanadium precipitation to obtain ammonium polyvanadate with a water content of 45wt%; the ammonium sulfate addition coefficient is 1.25;

[0106] The ammonium polyvanadate is dried at 350°C, then calcined at 500°C for deammoniation, and melted at 1050°C to obtain the vanadium pentoxide.

[0107] Example 4

[0108] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0109] In this embodiment, the iron content of the vanadium slag in step (1) is adjusted to 5 wt%.

[0110] Example 5

[0111] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0112] In this embodiment, the particle size range of the refined vanadium slag in step (1) is adjusted to 160-200 mesh.

[0113] Example 6

[0114] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0115] In this embodiment, the calcination time in step (2) is adjusted to 240 minutes.

[0116] Example 7

[0117] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0118] In this embodiment, the amount of sodium carbonate added in step (2) is adjusted to 25% of the mass of the refined vanadium slag, and the amount of sodium chloride added is adjusted to 75% of the mass of the refined vanadium slag.

[0119] Example 8

[0120] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0121] In this embodiment, the terminal temperature of the sodium calcination in step (2) is adjusted to 750°C.

[0122] Example 9

[0123] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0124] In this embodiment, the terminal temperature of the sodium calcination in step (2) is adjusted to 950°C.

[0125] Example 10

[0126] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0127] In this embodiment, the laying height difference between the refractory material and the castable material in step (2) is adjusted to 0 mm.

[0128] Embodiment 11

[0129] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0130] In this embodiment, the phosphorus removal process described in step (3) is omitted.

[0131] Example 12

[0132] This embodiment provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from that of embodiment 1 only in that:

[0133] In this embodiment, the endpoint of the mixed sulfuric acid in the vanadium precipitation treatment in step (3) is adjusted to a pH value of 3.

[0134] Comparative Example 1

[0135] This comparative example provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from Example 1 only in that:

[0136] In this comparative example, the magnetic separation and air separation processes for removing iron and impurities in step (1) are omitted.

[0137] Comparative Example 2

[0138] This comparative example provides a method for preparing vanadium pentoxide using high-chromium vanadium slag, and the method is different from Example 1 only in that:

[0139] In this comparative example, the sodium-forming roasting in the roasting treatment of step (2) is adjusted to calcium-forming roasting, that is, the sodium carbonate and sodium chloride are adjusted to the same mass of calcium carbonate.

[0140] After testing and calculation, the vanadium recovery rate and the purity of vanadium pentoxide using the methods provided in the above embodiments and comparative examples are shown in Table 1.

[0141] Table 1

[0142]

[0143]

[0144] From Table 1, we can see the following points:

[0145] (1) Comprehensive analysis of Examples 1-3 shows that the method provided by the present invention can achieve efficient vanadium extraction from high-chromium vanadium slag to obtain vanadium pentoxide with high purity;

[0146] (2) Comprehensive analysis of Examples 1, 4-5 and Comparative Example 1 shows that the magnetic separation and impurity removal, wind separation and grinding in step (1) can adjust the particle size range and iron content of the refined vanadium slag, thereby affecting the vanadium recovery rate in the subsequent process. This shows that the iron and impurity removal process in step (1) is one of the important factors affecting the vanadium recovery rate;

[0147] (3) Comprehensive analysis of Example 1 and Examples 6, 8-9 shows that reducing the roasting time will lead to low recovery rate; too high sodium roasting temperature will lead to ring formation in the kiln, affecting the recovery rate and purity (such as Example 9); too low sodium roasting temperature will lead to low vanadium conversion rate and low recovery rate (such as Example 8);

[0148] (4) Comprehensive analysis of Example 1 and Example 10 shows that when the laying height difference between the refractory material and the castable material is adjusted to 0 mm, the lifting plate inside the rotary kiln cannot function, which affects the full contact effect between the material and oxygen, resulting in a decrease in the vanadium nurturing effect, a low conversion rate, and a lower recovery rate;

[0149] (5) Comprehensive analysis of Example 1 and Comparative Example 2 shows that, compared with sodium roasting, calcium roasting leads to lower yield, higher cost and lower recovery rate.

[0150] In summary, the method provided by the present invention can effectively solve the problem of low vanadium conversion rate in clinker caused by increased chromium content in vanadium slag; the method effectively improves the recovery rate of vanadium and reduces costs.

[0151] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing vanadium pentoxide using high chromium vanadium slag, characterized in that: The method comprises the following steps: (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron, grinding, and air separation to remove impurities, to obtain refined vanadium slag; (2) mixing the sodium salt and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln to obtain clinker; (3) The clinker obtained in step (2) is wet-grinded and post-treated to obtain the vanadium pentoxide.

2. The method according to claim 1, characterized in that The high chromium-vanadium slag in step (1) has a chromium content of 8-12 wt% in terms of Cr2O3, a vanadium content of 12-15 wt% in terms of V2O5, and an iron content of 15-18 wt% in terms of elemental iron; Preferably, the magnetic field strength of the magnetic separation and iron removal in step (1) is 50-70 mT; Preferably, the grinding process in step (1) comprises coarse ball milling and fine ball milling performed sequentially; Preferably, the pressure of the air separation and impurity removal in step (1) is 2.5 to 3.5 kPa; Preferably, the iron content in the vanadium slag in step (1) is 1.5-3wt%; Preferably, the particle size of the refined vanadium slag in step (1) is in the range of 100 to 150 meshes.

3. The method according to claim 1 or 2, characterized in that: The sodium salt in step (2) includes sodium carbonate and sodium chloride; Preferably, the amount of sodium carbonate added is 70-80% of the mass of the refined vanadium slag; Preferably, the amount of sodium chloride added is 20-30% of the mass of the refined vanadium slag.

4. The method according to any one of claims 1 to 3, characterized in that: The rotating speed of the rotary kiln is 0.3-0.68 r / min; Preferably, refractory materials are laid at intervals on the inner wall of the rotary kiln; Preferably, castables are laid between adjacent refractory materials; Preferably, the distance between adjacent refractory materials is 180 to 220 mm; Preferably, the laying height difference between the refractory material and the castable material is 10 to 15 mm.

5. The method according to any one of claims 1 to 4, characterized in that: The calcination time in step (2) is 260 to 300 minutes; Preferably, the roasting treatment in step (2) comprises oxidation roasting, sodium roasting and cooling treatment performed in sequence; Preferably, the terminal temperature of the oxidative roasting is 600-700°C; Preferably, the terminal temperature of the sodium roasting is 800-850°C; Preferably, the terminal temperature of the cooling treatment is 550-600°C.

6. The method according to any one of claims 1 to 5, characterized in that: The solid-to-liquid ratio of clinker to water in the wet grinding of step (3) is 1:2.5-3.5; Preferably, the wet grinding time in step (3) is 3 to 5 minutes; Preferably, the wet grinding in step (3) also includes a cooling process after exiting the furnace.

7. The method according to any one of claims 1 to 6, characterized in that: The post-treatment in step (3) comprises: sequentially performing leaching filtration and vanadium precipitation treatment to obtain ammonium polyvanadate, and then sequentially performing drying treatment, calcination deammoniation and melting treatment to obtain the vanadium pentoxide.

8. The method according to claim 7, characterized in that The vanadium precipitation treatment comprises: mixing calcium chloride and the filtrate obtained by leaching and filtering to remove phosphorus, leaving the mixture to stand to obtain a supernatant, and then mixing the supernatant, sulfuric acid and ammonium salt to precipitate vanadium; Preferably, the amount of calcium chloride added is 0.014-0.018 wt% of the mass of the filtrate; Preferably, the standing time is 12 to 24 hours; Preferably, the water content of the ammonium polyvanadate is 35-45 wt %.

9. The method according to claim 7, characterized in that: The temperature of the drying process is 300-350°C; Preferably, the calcination deamination temperature is 400-600°C; Preferably, the temperature of the melting treatment is 820-1050°C.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) crushing the high-chrome vanadium slag, performing magnetic separation to remove iron at a magnetic field strength of 50 to 70 mT, and then performing coarse ball milling and fine ball milling, and then performing air separation to remove impurities at a pressure of 2.5 to 3.5 kPa to obtain refined vanadium slag with an iron content of 1.5 to 3 wt% and a particle size range of 100 to 150 mesh; The high chromium-vanadium slag has a chromium content of 8-12 wt% in terms of Cr2O3, a vanadium content of 12-15 wt% in terms of V2O5, and an iron content of 15-18 wt% in terms of elemental iron; (2) mixing sodium carbonate, sodium chloride and the refined vanadium slag obtained in step (1), and then roasting the mixture in a rotary kiln for 260 to 300 minutes and then cooling the mixture to obtain clinker; The amount of sodium carbonate added is 70-80% of the mass of the refined vanadium slag, and the amount of sodium chloride added is 20-30% of the mass of the refined vanadium slag; The rotation speed of the rotary kiln is 0.3-0.68 r / min. Refractory materials are laid on the inner wall of the rotary kiln at intervals, and castables are laid between adjacent refractory materials; the spacing between adjacent refractory materials is 180-220 mm; the laying height difference between the refractory materials and the castables is 10-15 mm; The roasting treatment includes oxidation roasting, sodium roasting and cooling treatment performed in sequence; the end temperature of the oxidation roasting is 600-700°C, the end temperature of the sodium roasting is 800-850°C, and the end temperature of the cooling treatment is 550-600°C; (3) mixing clinker and water at a solid-liquid ratio of 1:2.5-3.5 for wet grinding for 3-5 minutes, leaching and filtering, mixing calcium chloride and the filtrate obtained by leaching and filtering for phosphorus removal, standing for 12-24 hours to obtain a supernatant, and then mixing the supernatant, sulfuric acid and ammonium salt for vanadium precipitation treatment to obtain ammonium polyvanadate with a water content of 35-45wt%; The ammonium polyvanadate is dried at 300-350°C, then calcined at 400-500°C for deammoniation, and melted at 820-1050°C to obtain the vanadium pentoxide.

Citation Information

Cited By

  • A method for preparing chromium trioxide and vanadium pentoxide using chromium-vanadium-containing slag

    CN119750648A