Layered oxide precursor for sodium ion battery positive electrode material as well as preparation method and application of layered oxide precursor
By using a co-precipitation method with EDDHA-Na as a complexing agent and alkali as a precipitant to prepare precursors for sodium-ion battery cathode materials, the problems of poor particle sphericity and uneven element distribution were solved, thereby improving electrochemical performance and material uniformity.
Patent Information
- Application Number
- CN202410814270.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-12
AI Technical Summary
Existing methods for preparing precursors for sodium-ion battery cathode materials suffer from problems such as poor particle sphericity, easy agglomeration, and uneven element distribution, which affect electrochemical performance.
Ethylenediamine di-o-phenylacetic acid sodium salt (EDDHA-Na) was used as a complexing agent, combined with an alkali as a precipitant, to control the precipitation process of metal elements and regulate the morphology and particle size distribution of precursor particles, thereby preparing layered oxide precursors by co-precipitation.
This resulted in precursor particles with excellent morphology and uniform particle size distribution, improved electrochemical performance, shortened sodium ion conduction radius, and increased internal porosity and looseness of secondary particles.
Smart Images

Figure CN118929780A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion battery materials, and mainly relates to a layered oxide precursor for a sodium ion battery positive electrode material, and a preparation method and application thereof. Background Art
[0002] The sodium-ion battery system has the characteristics of abundant resources and low price, as well as similar electrochemical properties to the lithium-ion battery system. In recent years, it has received widespread attention in the fields of energy storage and low-speed electric vehicles. The sodium-ion positive electrode materials on the market are divided into three categories: layered transition metal oxides, polyanion compounds, and Prussian blue. Among them, layered oxide positive electrode materials have the advantages of high energy density, low cost, fast charging, and low-temperature performance. They are suitable for low-speed passenger cars and two-wheeled vehicles, and are the mainstream positive electrode materials for current sodium-ion batteries.
[0003] Common preparation methods for precursors of layered oxide positive electrode materials include high-temperature calcination and co-precipitation. Among them, the high-temperature calcination method is to directly mix and sinter various metal oxides with sodium salts at high temperature. This method has high preparation costs, uneven products, and difficult to control morphology. The synthesis process of the co-precipitation method is relatively complicated compared to the high-temperature calcination method, but the product uniformity is better, the morphology is easier to control, the synthesis cost is lower, and the energy consumption is less. It is currently the mainstream process for synthesizing precursors of sodium positive electrode materials.
[0004] At present, the preparation of sodium ion positive electrode material precursors is not only conventional ternary materials, but also the addition of other elements such as copper and zinc. For example, patent CN109037671A discloses a copper-iron-manganese / nickel layered oxide precursor for sodium ion batteries and its preparation method and use, wherein the copper source, iron source and manganese source are prepared into a salt solution according to a preset ratio; or the copper source, iron source, manganese source and nickel source are prepared into a salt solution according to a preset ratio; then the prepared salt solution is added dropwise to the sodium hydroxide solution, and the reaction products obtained above are cooled in turn, solid-liquid separation is performed, and the water washing liquid is washed until it is neutral and dried to obtain the precursor product. The obtained precursor particles have poor sphericity, and the balls are easily adhered together, and structural cracks are easily generated during the sintering of the positive electrode, which affects the electrochemical performance. Moreover, the difference in the solubility product constants of different metal elements will lead to uneven distribution of the elements of the precursor material, thereby affecting the performance of the battery material. The selection of a suitable complexing agent is of great significance for the preparation of the precursor material.
[0005] Patent application with publication number CN116621235A discloses a method for preparing a nickel-iron-copper-manganese precursor, comprising: 2+ , Fe 2+ , Mn 2+ Cu 2+React with a precipitating agent and a complexing agent in a solution system to form a quaternary precursor of nickel-iron-copper-manganese hydroxide; the complexing agent is sodium citrate; the precipitating agent is a base. The disclosed nickel-iron-copper-manganese precursor is prepared by the above method. The disclosed cathode material is obtained by sintering the above precursor and a sodium source. The disclosed cathode uses the above cathode material. The disclosed sodium-ion battery includes the above cathode. The precursor prepared by the preparation method provided by the invention has a good microscopic morphology and good electrochemical performance after being made into a cathode material. However, there are still defects in the microscopic appearance and electrochemical performance.
[0006] In view of this, the present invention is specifically proposed. Summary of the Invention
[0007] Aiming at the deficiencies of the existing technology, the purpose of the present invention is to provide a layered oxide precursor for a sodium-ion battery cathode material, its preparation method and application. The prepared precursor material has excellent morphology, uniform and controllable particle size distribution, and good electrochemical performance.
[0008] To achieve this purpose, the present invention adopts the following technical solutions:
[0009] The present invention provides a preparation method of a layered oxide precursor for a sodium-ion battery cathode material. The chemical formula of the layered oxide precursor is Ni x Fe y Cu z Mn w CO3 or Ni x Fe y Cu z Mn w (OH)2, x + y + z + w = 100, 0 < x < 33.3, 0 ≤ y ≤ 45, 0 ≤ z < 20, 0 < w < 33.3, which is a low-nickel layered oxide precursor.
[0010] React a metal salt solution, a complexing agent and a precipitating agent to form the layered oxide precursor.
[0011] The complexing agent is sodium ethylenediamine di(o-phenylacetate) (EDDHA-Na);
[0012] The precipitating agent is a base;
[0013] The preparation method specifically includes:
[0014] Continuously introduce a metal salt solution, a complexing agent and a precipitating agent into a reaction kettle, react under an inert gas to obtain a reaction product, and subject the reaction product to a washing treatment to finally obtain the layered oxide precursor.
[0015] Among them, the value of x can be 0, 10, 25, 33.3, and other values not listed in this range are also applicable. When x is 0, it means that the precursor of the sodium ion layer oxygen positive electrode material does not contain nickel element; the value of y can be 0, 30, 33.3, 45, and other values not listed in this range are also applicable; the value of z can be 0, 20; the value of w can be 30, 33.3, and other values not listed in this range are also applicable.
[0016] The metal salt solution is prepared from a nickel source, an iron source and a manganese source according to a set ratio, or a nickel source, an iron source, a copper source and a manganese source according to a set ratio.
[0017] In some embodiments of the present invention, the concentration of the metal salt solution is 1-3 mol / L. It can be 0.75 mol / L, 1 mol / L, 1.5 mol / L, including but not limited to the above-listed concentration ranges; the concentration of the precipitant is 3-5 mol / L, the concentration of the complexing agent is 5-30 g / L; the precipitant is at least one of sodium hydroxide and sodium carbonate. The complexing agent is not added alone, but the complexing agent EDDHA-Na is added to the prepared precipitant solution.
[0018] In some embodiments of the present invention, the pH of the bottom liquid in the reactor is 10.5-12.2, the temperature of the bottom liquid in the reactor is 50-60°C, and the concentration of the complexing agent in the bottom liquid in the reactor is 0.5-3 g / L. In the embodiment of the present invention, the pH of the bottom liquid in the reactor is 11.5-12.2, the temperature of the bottom liquid in the reactor is 55-60°C, and the concentration of the complexing agent in the bottom liquid in the reactor is 0.67 g / L as an example, but it is not limited thereto.
[0019] In some embodiments of the present invention, the feed rate of the metal salt solution in the reaction is 3-5 ml / min, the feed rate of the precipitant is 1-3 ml / min, and the feed rate of the complexing agent is 0.1-0.5 ml / min.
[0020] In some embodiments of the present invention, the reaction conditions are: the reaction pH is 9-12, the reaction temperature is 40-60°C; the reaction is carried out under double-layer impeller stirring, and the stirring speed is 800-1000rpm.
[0021] In some embodiments of the present invention, the particle size growth rate of the layered oxide precursor is controlled between 0.02-0.08 μm / h until the layered oxide precursor grows to a D50 of 3-8 μm and the reaction is stopped. It can be 4, 5, 6, 8 μm, including but not limited to the listed particle size values.
[0022] In some embodiments of the present invention, the material washing treatment is carried out by filtering with a filter to obtain a filter cake, washing it three times with pure water, and drying it at 80-120°C after washing.
[0023] In some embodiments of the present invention, the metal salt solution further includes a stabilizer, which is sulfuric acid, and 5 to 6 ml of the stabilizer with a mass fraction of 50% is added per liter of the metal salt solution.
[0024] The present invention also provides a layered oxide precursor for a sodium ion battery positive electrode material, which is prepared by the above-mentioned preparation method.
[0025] The present invention also provides a positive electrode, comprising a positive electrode material, wherein the positive electrode material is prepared by mixing the above-mentioned layered oxide precursor with a sodium source and then sintering the mixture.
[0026] The present invention also provides a sodium ion battery, comprising the above-mentioned positive electrode.
[0027] The present invention has the following beneficial effects:
[0028] The preparation method of the sodium ion battery positive electrode material precursor provided by the present invention is different from the common ammonia water and sodium citrate as the complexing agent. EDDHA-Na is selected as the single complexing agent, which can better control the uniform precipitation of metal elements. The precursor particles have good morphology and small primary particle size, which can shorten the sodium ion conduction radius and increase the internal looseness and porosity of the secondary particles. The positive electrode material prepared by the precursor has good electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The electron microscope morphology image (A) and particle size image (B) of the precursor particles prepared in Example 1.
[0030] Figure 2 (A) and (B) are electron microscope morphology images and particle size images of the precursor particles prepared in Example 2.
[0031] Figure 3 (A) and (B) the electron microscope morphology image of the precursor particles prepared in Example 3.
[0032] Figure 4 The electron microscope morphology image (A) and particle size image (B) of the precursor particles prepared in Comparative Example 1.
[0033] Figure 5 The electron microscope morphology image (A) and particle size image (B) of the precursor particles prepared in Comparative Example 2.
[0034] Figure 6 (A) and (B) are the electron microscope morphology images and particle size images of the precursor particles prepared in Comparative Example 3.
[0035] Figure 7 The electron microscope morphology image (A) and particle size image (B) of the precursor particles prepared in Comparative Example 4. DETAILED DESCRIPTION
[0036] Example 1
[0037] This embodiment provides a method for preparing a precursor of a positive electrode material for a sodium ion battery, comprising Ni 33 .3Fe 33 .3Mn 333 (OH) 2, the preparation method comprises the following steps:
[0038] (1) Preparation of reaction raw materials
[0039] Nickel sulfate, ferrous sulfate and manganese sulfate are mixed in a molar ratio of 33.3:33.3:33.3, and pure water is added to prepare a mixed metal salt solution with a total metal concentration of 1 mol / L. 5 ml of 50% sulfuric acid is added per liter of salt solution as a stabilizer to prevent oxidation of divalent iron ions, and the pH value of the mixed salt solution can be around 2.0.
[0040] 5 mol / L sodium hydroxide was prepared as a precipitant solution, and 10 g of EDDHA-Na was added as a complexing agent per liter of the sodium hydroxide precipitant solution to prepare a mixed solution of the precipitant and the complexing agent.
[0041] (2) Preparation of reaction base solution
[0042] Under nitrogen atmosphere protection and stirring speed of 400 rpm, 3 L of pure water, 200 g of sodium sulfate and 2 g of EDDHA-Na were added to a 5 L reactor, the temperature was raised to maintain 55° C., and sodium hydroxide aqueous solution was added to adjust the pH to 11.5.
[0043] (3) Coprecipitation reaction
[0044] The salt solution in the above step (1) is fed into the reactor at a feeding rate of 4 ml / min, and the precipitant and complexing agent solutions are added at the same time. After the coprecipitation reaction is carried out for 2 hours at a stirring speed of 900 rpm and an inert gas protective atmosphere, the pH is lowered to 10.5 and the reaction is continued until the reaction is completed. The feeding rate of the precipitant and complexing agent mixed solution is automatically adjusted between 1-3 ml / min, and the growth rate of the precursor particle size is controlled between 0.02-0.08 μm / h. When the precursor particle size D50 grows to about 5 μm, the feeding is stopped.
[0045] (4) Post-processing of washed materials
[0046] The collected overflow slurry and the slurry in the reactor are mixed evenly, placed in a filter for suction filtration, washed three times with ultrapure water, and then the filter cake is placed in a 120°C oven for drying. After sieving, the precursor product can be obtained. The electron microscopy morphology and particle size of the precursor particles are shown in Figure 1 As shown, the particles have good sphericity, uniform size, and the primary grains have an obvious staggered structure.
[0047] Example 2
[0048] This embodiment provides a method for preparing a precursor of a positive electrode material for a sodium ion battery, comprising Ni 33 .3Fe 33 .3Mn 333 (OH)2, except that the concentration of the mixed metal salt solution was 1.5 mol / L and the amount of the complexing agent EDDHA-Na was increased to 30 g, the rest was the same as in Example 1. The electron microscopic morphology and particle size of the precursor particles are shown in Figure 2 As shown, the electron microscope morphology is similar to that of Example 1, but the primary grain development is relatively poor.
[0049] Example 3
[0050] This embodiment provides a method for preparing a precursor of a positive electrode material for a sodium ion battery, comprising Ni 33 .3Fe 33 .3Mn 333 (OH)2, except that the reaction temperature was adjusted to 60°C and the amount of complexing agent EDDHA-Na was adjusted to 5g, the rest was the same as in Example 1. The electron microscopic morphology and particle size of the precursor particles are shown in Figure 3 As shown, compared with the electron microscopy morphology of Example 1, the sphericity is slightly worse, but there are also obvious staggered primary grains.
[0051] Comparative Example 1
[0052] This comparative example provides a method for preparing a sodium ion battery positive electrode material precursor, which is composed of Ni 33 .3Fe 33 .3Mn 333 (OH) 2, the preparation method comprises the following steps:
[0053] (1) Preparation of reaction raw materials
[0054] Nickel sulfate, ferrous sulfate and manganese sulfate are mixed in a molar ratio of 33.3:33.3:33.3, and pure water is added to prepare a mixed metal salt solution with a total metal concentration of 1 mol / L. 5 ml of 50% sulfuric acid is added per liter of salt solution as a stabilizer to prevent oxidation of divalent iron ions, and the pH value of the mixed salt solution can be around 2.0.
[0055] 5 mol / L sodium hydroxide was prepared as a precipitant solution and 12.5% ammonia water was prepared as a complexing agent.
[0056] (2) Preparation of reaction base solution
[0057] Under nitrogen atmosphere protection and stirring speed of 400 rpm, 3 L of pure water, 200 g of sodium sulfate and 108 g of 12.5% ammonia water were added to a 5 L reactor, the temperature was maintained at 60° C., and alkali solution was added to adjust the pH to 12.2.
[0058] (3) Coprecipitation reaction
[0059] The salt solution in the above step (1) is fed into the reactor at a feeding rate of 5 ml / min, and the precipitant and complexing agent solutions are added at the same time. After the coprecipitation reaction is carried out for 2 hours at a stirring speed of 1000 rpm and an inert gas protective atmosphere, the pH is lowered to 11 and the reaction is continued until the reaction is completed. The feeding rate of the precipitant is automatically adjusted between 1.5-3.2 ml / min, and the feeding rate of the complexing agent is 0.35 ml / min. The growth rate of the precursor particle size is controlled between 0.03-0.06 μm / h. When the precursor particle size D50 grows to about 6 μm, the feeding is stopped.
[0060] (4) Post-processing of washing materials
[0061] The collected overflow slurry and the slurry in the reactor are mixed evenly, placed in a filter for suction filtration, washed three times with ultrapure water, and then the filter cake is placed in a 120°C oven for drying. After sieving, the precursor product can be obtained. The morphology and particle size of the precursor particles are as follows Figure 4 As shown, the particles have a certain sphericity, but the size is uneven.
[0062] Comparative Example 2
[0063] This comparative example provides a method for preparing a sodium ion battery positive electrode material precursor, which is composed of Ni 25 Fe 45 Mn 30 (OH) 2, the preparation method comprises the following steps:
[0064] (1) Preparation of reaction raw materials
[0065] Nickel sulfate, ferrous sulfate and manganese sulfate are mixed in a molar ratio of 25:45:30, and pure water is added to prepare a mixed metal salt solution with a total metal concentration of 1 mol / L. 6 ml of 50% sulfuric acid is added per liter of salt solution as a stabilizer to prevent oxidation of divalent iron ions. The pH value of the mixed salt solution can be around 1.8.
[0066] 3 mol / L sodium hydroxide was prepared as a precipitant solution, and 5 g of sodium citrate was added as a complexing agent per liter of the sodium hydroxide solution to prepare a mixed solution of the precipitant and the complexing agent.
[0067] (2) Preparation of reaction base solution
[0068] Under nitrogen atmosphere protection and stirring speed of 400 rpm, 3 L of pure water, 300 g of sodium sulfate and 2 g of sodium citrate were added to a 5 L reactor, the temperature was raised to maintain 55°C, and sodium hydroxide aqueous solution was added to adjust the pH to 12.
[0069] (3) Coprecipitation reaction
[0070] The salt solution in the above step (1) is fed into the reactor at a feeding rate of 4 ml / min, and the precipitant and complexing agent solutions are added at the same time. After the coprecipitation reaction is carried out for 2 hours at a stirring speed of 1000 rpm and an inert gas protective atmosphere, the pH is lowered to 10.8 and the reaction is continued until the reaction is completed. The feeding rate of the precipitant and complexing agent mixed solution is automatically adjusted between 1-3 ml / min, and the growth rate of the precursor particle size is controlled between 0.02-0.08 μm / h. When the precursor particle size D50 grows to about 6 μm, the feeding is stopped.
[0071] (4) Post-processing of washed materials
[0072] The collected overflow slurry and the slurry in the reactor are mixed evenly, placed in a filter for suction filtration, washed three times with ultrapure water, and then the filter cake is placed in a 120°C oven for drying. After sieving, the precursor product can be obtained. The electron microscopy morphology and particle size of the precursor particles are shown in Figure 5 As shown, the particles have poor sphericity and agglomeration.
[0073] Comparative Example 3
[0074] This comparative example provides a method for preparing a sodium ion battery positive electrode material precursor, which is composed of Ni 25 Fe 45 Mn 30 (OH) 2, the preparation method comprises the following steps:
[0075] (1) Preparation of reaction raw materials
[0076] Nickel sulfate, ferrous sulfate and manganese sulfate are mixed in a molar ratio of 25:45:30, and pure water is added to prepare a mixed metal salt solution with a total metal concentration of 1 mol / L. 5 ml of 50% sulfuric acid is added per liter of salt solution as a stabilizer to prevent oxidation of divalent iron ions. The pH value of the mixed salt solution can be around 1.8.
[0077] Prepare 3 mol / L sodium hydroxide as a precipitant solution and 12.5% ammonia water as a complexing agent solution.
[0078] (2) Preparation of reaction base solution
[0079] Under nitrogen atmosphere protection and stirring speed of 400 rpm, 3 L of pure water, 300 g of sodium sulfate and 108 g of 12.5% ammonia water were added to a 5 L reactor, the temperature was maintained at 55°C, and sodium hydroxide aqueous solution was added to adjust the pH to 12.
[0080] (3) Coprecipitation reaction
[0081] The salt solution in the above step (1) is fed into the reactor at a feeding rate of 4 ml / min, and the precipitant and complexing agent solutions are added at the same time. After the coprecipitation reaction is carried out for 2 hours at a stirring speed of 1000 rpm and an inert gas protective atmosphere, the pH is lowered to 10.8 and the reaction is continued until the reaction is completed. The feeding rate of the precipitant is automatically adjusted between 1-3.2 ml / min, and the feeding rate of the complexing agent is 0.3 ml / min. The growth rate of the precursor particle size is controlled between 0.02-0.05 μm / h. When the precursor particle size D50 grows to about 8 μm, the feeding is stopped.
[0082] (4) Post-processing of washing materials
[0083] The collected overflow slurry and the slurry in the reactor are mixed evenly, placed in a filter for suction filtration, washed three times with ultrapure water, and then the filter cake is placed in a 120°C oven for drying. After sieving, the precursor product can be obtained. The electron microscopy morphology and particle size of the precursor particles are shown in Figure 6 shown.
[0084] Comparative Example 4
[0085] This comparative example provides a method for preparing a sodium ion battery positive electrode material precursor, which is composed of Ni 11.1 Fe 33.3 Cu 22.2 Mn 33.3 CO3, the preparation method comprises the following steps:
[0086] (1) Preparation of reaction raw materials
[0087] Mix nickel sulfate, ferrous sulfate, copper sulfate and manganese sulfate in a molar ratio of 10:30:20:30, add pure water, and prepare a mixed metal salt solution with a total metal concentration of 1 mol / L. Add 5 ml of 50% sulfuric acid per liter of solution as a stabilizer to prevent oxidation of divalent iron ions. The pH value of the mixed salt solution can be around 2.0.
[0088] Prepare 1 mol / L sodium carbonate as a precipitant solution.
[0089] 8 g / L sodium citrate was used as the complexing agent solution.
[0090] (2) Preparation of reaction base solution
[0091] Under nitrogen atmosphere protection and stirring speed of 400 rpm, 3 L of pure water, 300 g of sodium sulfate and 1 g of sodium citrate were added to a 5 L reactor, the temperature was raised to maintain at 50°C, and sodium carbonate was added to adjust the pH to 12.
[0092] (3) Coprecipitation reaction
[0093] The salt solution in the above step (1) is fed into the reactor at a feeding rate of 3 ml / min, and the precipitant and complexing agent solutions are added at the same time. After the coprecipitation reaction is carried out for 2 hours at a stirring speed of 1000 rpm and an inert gas protective atmosphere, the pH is lowered to 10.8 and the reaction is continued until the reaction is completed. The feeding rate of the precipitant is automatically adjusted between 3-6 ml / min, and the feeding rate of the complexing agent is 1.5 ml / min. The growth rate of the precursor particle size is controlled between 0.02-0.06 μm / h. When the precursor particle size D50 grows to about 8 μm, the feeding is stopped.
[0094] (4) Post-processing of washed materials
[0095] The collected overflow slurry and the slurry in the reactor are mixed evenly, placed in a filter for suction filtration, washed three times with ultrapure water, and then the filter cake is placed in a 120°C oven for drying. After sieving, the precursor product can be obtained. The electron microscopy morphology and particle size of the precursor particles are shown in Figure 7 As shown, the particle shape is uneven and the primary grain development is poor.
[0096] Test Example 1
[0097] The precursors prepared in the above embodiments and comparative examples were placed in a mixer and mixed with sodium carbonate respectively, wherein the mixing ratio of sodium ions to precursor metal elements was 0.96:1, and the mixture was sintered in an atmosphere furnace at 800°C for 10 hours and naturally cooled to room temperature to obtain the corresponding positive electrode material.
[0098] The above positive electrode materials were assembled into a half-button battery to test its electrochemical performance. Among them, the mass ratio of positive electrode material to conductive agent (carbon black) and binder (PVDF) was 95:5:5. The mixture was placed in a vacuum mixer for stirring, and the evenly stirred slurry was coated on aluminum foil. After drying, rolling and slicing, the corresponding positive electrode material pole piece was obtained. Sodium sheet was used as negative electrode sheet, 1 mol / L sodium hexametaphosphate solution was used as electrolyte, and PC (polypropylene diaphragm) was used as diaphragm. After making a half-button battery in a glove box, the performance test was performed. The results of the electrochemical performance test are shown in the following table.
[0099]
[0100] In summary, in the method for preparing a precursor of anode material for sodium ion battery proposed in the present invention, compared with conventional chelating agents ammonia water and sodium citrate, selecting EDDHA-Na as a chelating agent can better regulate the nucleation and growth of crystals. The prepared precursor has a simple production process, good uniformity of metal element precipitation, excellent electron microscope morphology and structure, and a relatively uniform particle size distribution.
Claims
1. A method for preparing a layered oxide precursor for a sodium ion battery positive electrode material, characterized in that: The chemical formula of the layered oxide precursor is Ni x Fe y Cu z Mn w CO3 or Ni x Fe y Cu z Mn w (OH)2, x+y+z+w=100, 0≤x≤33.3, 0≤y≤45, 0≤z≤20, 0≤w≤33.3, reacting a metal salt solution, a complexing agent and a precipitant to generate the layered oxide precursor; The complexing agent is sodium ethylenediamine di-o-phenylacetate; The precipitant is a base; The preparation method specifically comprises: The metal salt solution, the complexing agent and the precipitant are continuously introduced into the reaction kettle to react under an inert gas to obtain a reaction product, and the reaction product is subjected to a material washing treatment to finally obtain the layered oxide precursor.
2. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The metal ion concentration of the metal salt solution is 1-3 mol / L, The concentration of the precipitant is 3-5 mol / L. The concentration of the complexing agent is 5 to 30 g / L; The precipitant is at least one of sodium hydroxide and sodium carbonate.
3. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The pH of the bottom liquid in the reaction kettle is 10.5-12.2, the temperature of the bottom liquid in the reaction kettle is 50-60° C., and the concentration of the complexing agent in the bottom liquid in the reaction kettle is 0.5-3 g / L.
4. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The feed rate of the metal salt solution in the reaction is 3-5 ml / min. The feeding rate of the precipitant is 1-3 ml / min, The feeding rate of the complexing agent is 0.1-0.5 ml / min.
5. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The reaction conditions are: the reaction pH is 9-12, the reaction temperature is 40-60°C; The reaction is carried out under stirring with a double-layer impeller, and the stirring speed is 800-1000 rpm.
6. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The particle size growth rate of the layered oxide precursor is controlled to be between 0.02-0.08 μm / h, and the reaction is stopped until the layered oxide precursor grows to a D50 of 3-8 μm.
7. The method for preparing a layered oxide precursor for a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The method of the material washing treatment is: using a filter to filter to obtain a filter cake, then washing it three times with pure water, and drying it at 80-120°C after washing.
8. A layered oxide precursor for a sodium ion battery positive electrode material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. A positive electrode, characterized in that The positive electrode material comprises a positive electrode material, wherein the positive electrode material is prepared by mixing the layered oxide precursor according to claim 8 with a sodium source and then sintering the mixture.
10. A sodium ion battery, characterized in that: Comprising the positive electrode as claimed in claim 9.
Citation Information
Patent Citations
Sodium-ion battery positive electrode material precursor, preparation method thereof and positive electrode material
CN117023661A
Sodium-ion battery positive electrode material precursor as well as preparation method and application thereof