High-nickel ternary oxide material and preparation method and application thereof

High nickel ternary oxide materials were prepared by sol-gel method, and citric acid was used to promote uniform dispersion of metal ions, solving the structural mixing and side reaction problems of high nickel NCM811 positive electrode materials, and improving the electrochemical performance and cycle stability of the battery sex.

CN118929789APending Publication Date: 2024-11-12NANCHANG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208312.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The high-nickel NCM811 positive electrode material has structural mixing and surface side reactions, which hinders the full performance of the battery's electrochemical performance and has irreversible side effects on the cycle performance.

Method used

The high-nickel ternary oxide material is prepared by sol-gel method. Citric acid is used as a chelating agent and complexing agent to adjust the pH value and temperature to form a stable chelate, prevent direct reaction between ions, and promote uniform dispersion of the material structure. and stability.

Benefits of technology

It improves the purity and structural stability of the material, reduces the degree of mixing between Ni2+ and Li+, enhances the contact between the electrolyte and the active material, and improves the lithium storage and circulation performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929789A_ABST
    Figure CN118929789A_ABST
Patent Text Reader

Abstract

The invention discloses a high-nickel ternary oxide material and a preparation method and application thereof, and belongs to the technical field of battery electrode materials, citric acid is used as a complexing agent and a chelating agent, and metal ions can be promoted to form stable chelate, so that direct reaction among the ions is prevented, and generation of precipitates is prevented; in addition, the metal ions serve as a network forming agent in the gel forming process, so that the metal ions are uniformly dispersed in a gel network, and stable formation of a material structure is further promoted through high-temperature oxygen atmosphere calcination. The morphology of the material is regulated and controlled by controlling the reaction solvent, the reaction temperature and the reaction pH value used in the gel-sol reaction process and the reaction temperature and the reaction time in the calcination process, and the particle size of the material is controlled in a proper range, so that on one hand, lithium ions can be deintercalated in a relatively short time; on the other hand, the particle size is proper, so that side reaction between electrolyte and an electrode is reduced, and the lithium storage performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery electrode materials, and in particular to a high-nickel ternary oxide material and a preparation method and application thereof. Background Art

[0002] In the past decade, researchers have developed nickel-rich and low-cobalt layered cathode materials with different nickel-cobalt contents. For example, Kim et al. 0.8 Co 0.2-x Mn x ](OH)2 and LiOH·H2O precursors, and spherical pure phase LiNi was synthesized for the first time. 0.8 Co 0.1 Mn 0.1 O2 (NCM811). NCM811 positive electrode material has a better performance than LiNi due to the addition of a small amount of Mn metal. 0.8 Co 0.2 O2 has better thermal stability and structural stability. Since then, NCM ternary materials have gradually attracted the attention of researchers due to their superior electrochemical properties, and have gradually developed into the mainstream choice of positive electrode materials for lithium-ion batteries on the market.

[0003] The theoretical energy density of NCM materials is about 600Wh kg -1 , the level of actual products has only developed about 35% of the theoretical limit. Therefore, in the future, automotive batteries may use a large number of NCM materials. In the field of power vehicles, lithium iron phosphate has good thermal stability compared with ternary materials. However, at present, new energy vehicles not only have safety and stability as a demand, but also high endurance is another important aspect. Therefore, as the positive electrode material that controls capacity and stability in the battery, it must have high specific capacity and energy density to solve the current endurance short board problem. And this is the advantage of ternary positive electrode materials.

[0004] At present, the domestic main cathode material is high-nickel NCM811, in which the high energy density brought by the high nickel content meets the endurance problem of the car. However, the high nickel content also brings many disadvantages, such as structural mixing and surface side reactions. The existence of these problems hinders the full play of its electrochemical performance and has irreversible side effects on the cycle performance. Summary of the invention

[0005] The present invention provides a high-nickel ternary oxide material and its preparation method and application, which effectively solves the technical problem that the existing high-nickel NCM811 as a positive electrode raw material has a mixed structure and surface side reactions that hinder the full play of the battery's electrochemical performance and cause irreversible side effects in the cycle performance. The present invention adopts a sol-gel method to prepare a high-nickel ternary oxide material to curb the appearance of impurities, so that the purity of the obtained material is relatively high. The Ni of the synthesized NCM811 2+ With Li + The degree of mixing is lower, the sample agglomeration is less, and the contact between the electrolyte and the active material is better.

[0006] The first object of the present invention is to provide a method for preparing a high-nickel ternary oxide material, characterized in that it comprises the following steps:

[0007] Using citric acid as a chelating agent, adding a mixed aqueous solution containing soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to the aqueous solution, mixing, adjusting the pH value to 4-9, stirring at 75-80° C. to combine the transition metal nickel ions, cobalt ions, manganese ions and lithium ions to form a chelate, and drying to obtain a xerogel;

[0008] The dry gel is crushed, and pre-calcined at 480-500° C. in an air atmosphere to decompose the acetate in the dry gel to obtain a precursor;

[0009] The precursor is heated to 700-800° C. and calcined in an oxygen atmosphere, so that the precursor gradually forms a layered structure and the crystal particles of the precursor are enlarged, thereby obtaining a high-nickel ternary oxide material.

[0010] As a preferred embodiment, the molar ratio of the soluble transition metal nickel salt, cobalt salt, manganese salt to the soluble lithium salt is 8:1:1:10.5.

[0011] As a preferred embodiment, the molar ratio of the sum of the soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to citric acid is 1:1.

[0012] As a preferred embodiment, the pre-calcination time is 180 min to 300 min.

[0013] As a preferred embodiment, the calcination time is 600 min to 900 min.

[0014] As a preferred embodiment, the oxygen flow rate in the oxygen atmosphere is 58-60 mL / min.

[0015] As a preferred embodiment, during drying, the drying process is performed at 200° C. to 250° C. for 180 min to 240 min.

[0016] The second object of the present invention is to provide a high-nickel ternary oxide material prepared by the above preparation method.

[0017] The third object of the present invention is to provide an application of the above-mentioned high-nickel ternary oxide material in the preparation of a positive electrode material for a lithium-ion battery, wherein the application is specifically as follows: a high-nickel ternary metal oxide material, a conductive agent and a binder are mixed in a mass ratio of 7 to 8:1 to 2:1, and then N-methylpyrrolidone is added to obtain a slurry, and an aluminum foil is used as a substrate, and the slurry is evenly coated on the surface of the substrate, and a positive electrode sheet of a lithium-ion battery is obtained after drying.

[0018] As a preferred embodiment, the conductive agent is conductive carbon black, carbon nanotubes or graphene, and the binder is polyvinylidene fluoride or carboxymethyl cellulose.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention provides a high-nickel ternary oxide material and a preparation method and application thereof, wherein a citric acid aqueous solution is added to a mixed aqueous solution containing a soluble transition metal nickel salt, a cobalt salt, a manganese salt and a soluble lithium salt, mixed, the pH value is adjusted to 4-9, stirred at 75-80°C, the transition metal nickel ions, cobalt and manganese ions are combined with lithium ions to form a chelate with a layered structure, dried to obtain a dry gel; the dry gel is crushed, pre-calcined at 480-500°C in an air atmosphere to obtain a precursor; the precursor is heated to 700-800°C and calcined in an oxygen atmosphere to obtain a high-nickel ternary oxide material. The present invention uses citric acid as a complexing agent and a chelating agent, which can promote the metal ions to form a stable chelate, thereby preventing direct reaction between ions and resulting in the formation of precipitation, and acts as a network former in the gel formation process, so that the metal ions are evenly dispersed in the gel network, and the material structure is further promoted to be stably formed by calcining in a high-temperature oxygen atmosphere.

[0021] 2. The preparation process of the high-nickel ternary oxide material of the present invention is simple, has no environmental pollution, is low in cost, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a morphology structure diagram of the high-nickel ternary metal oxide material prepared in Example 1 of the present invention;

[0023] Figure 2 This is an X-ray diffraction pattern of the high-nickel ternary metal oxide material prepared in Example 1 of the present invention;

[0024] Figure 3 This is a morphology structure diagram of the high-nickel ternary metal oxide material prepared in Example 3 of the present invention;

[0025] Figure 4 This is a morphology structure diagram of the high-nickel ternary metal oxide material prepared in Example 1 of the present invention;

[0026] Figure 5 This is a morphology structure diagram of the high-nickel ternary metal oxide material prepared in Example 2 of the present invention;

[0027] Figure 6 The morphology structure and element distribution diagram of the high-nickel ternary metal oxide material prepared in Example 1 of the present invention; wherein Figure A is the morphology structure diagram of the high-nickel ternary metal oxide material in Example 1, and Figures B, C and D are element distribution diagrams of the high-nickel ternary metal oxide material in Example 1;

[0028] Figure 7 The high nickel ternary metal oxide material prepared in Examples 1 to 3 of the present invention is subjected to a current density of 200 mAhg -1 The discharge performance diagram below;

[0029] Figure 8 The high nickel ternary metal oxide materials of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention are subjected to a current density of 200 mAh g -1 The discharge performance diagram below. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.

[0031] As mentioned in the background technology of the present invention, the domestic main raw material for positive electrode is high-nickel NCM811, wherein the higher nickel content can bring about high energy density, thereby meeting the endurance problem of the vehicle, but the high nickel content also brings about many disadvantages, such as structural mixing, irreversible phase change and surface side reactions. The existence of these problems hinders the full play of the electrochemical properties of batteries using high-nickel NCM811 as the positive electrode raw material, and also has irreversible side effects on the cycle performance. Based on the above technical problems, the present invention provides a high-nickel ternary oxide material and a preparation method and application thereof. The high-nickel ternary oxide material is prepared by a sol-gel method to curb the appearance of impurities, so that the purity of the obtained material is higher. The Ni of the synthesized NCM811 2+ With Li + The degree of mixing is lower, the sample agglomeration is less, and the contact between the electrolyte and the active material is better.

[0032] The technical contents of the present invention are analyzed and explained in detail below.

[0033] The present invention first provides a method for preparing a high-nickel ternary metal oxide material, comprising the following steps:

[0034] Using citric acid as a chelating agent, adding a mixed aqueous solution containing soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to the aqueous solution, mixing, adjusting the pH value to 4-9, stirring at 75-80° C. to combine the transition metal nickel ions, cobalt ions, manganese ions and lithium ions to form a chelate, and drying to obtain a xerogel;

[0035] The dry gel is crushed, and pre-calcined at 480-500° C. in an air atmosphere to decompose the acetate in the dry gel to obtain a precursor;

[0036] The precursor is heated to 700-800° C. and calcined in an oxygen atmosphere, so that the precursor gradually forms a phase and the crystal grains of the precursor are enlarged, thereby obtaining a high-nickel ternary oxide material.

[0037] In the above technical scheme, the technical principle is: using citric acid as a complexing agent and chelating agent to promote the metal ions nickel, cobalt, manganese and lithium to form stable chelates, thereby preventing direct reactions between ions and leading to the formation of precipitates, and acting as a network former in the gel formation process, so that the metal ions are evenly dispersed in the gel network, and the material structure is further promoted to be stably formed by calcining in a high-temperature oxygen atmosphere. The morphology of the material is regulated by controlling the reaction solvent, reaction temperature, reaction pH, and reaction temperature used in the gel sol reaction process, and the reaction temperature during the calcination process, and the particle size of the material is controlled within an appropriate range. The prepared high-nickel ternary oxide material is used to prepare positive electrode materials for lithium-ion batteries. On the one hand, lithium ions can be deintercalated in a relatively short time, and on the other hand, the appropriate particle size reduces side reactions between the electrolyte and the electrode, thereby improving the lithium storage performance. The high-nickel ternary oxide material prepared by the present invention curbs the appearance of impurities, so that the purity of the obtained material is relatively high, and the Ni of the synthesized NCM811 2+ With Li + The degree of mixing is lower, the sample agglomeration is less, and the contact between the electrolyte and the active material is better.

[0038] In order to ensure the formation of a chelate with a specific structure between metal ions, the molar ratio of the soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt is 8:1:1:10.5. Based on the molar ratio of the above metal ions, the final product with the molecular formula LiNi 0.8 Co 0.1 Mn 0.1 O2 chelate.

[0039] In order to effectively prevent the metal ions from reacting to form precipitation, thereby affecting the molecular structure of the chelate, the molar ratio of the sum of the soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to citric acid is 1: 1. If the amount of citric acid is reduced, the particle size of the final material is uneven. If the amount of citric acid is increased, the material structure is more unstable, affecting the crystallization performance of the material.

[0040] In order to fully decompose the acetate of the dry gel, the pre-calcination time is 180min to 300min. If the calcination is less than 180min at 480°C or below, the ion mixing degree of the cations is high, resulting in a large number of ion mixing defects remaining in the material crystal, and a large number of transition metal ions occupying lithium sites will seriously hinder the diffusion of lithium ions during the charge and discharge process. If the calcination is more than 300min at 500°C or above, the material particle size will be uneven.

[0041] In order to gradually form the precursor and increase the grain size in the precursor, the calcination time is 600min to 900min. If the calcination is less than 600min at 700℃ or below, the grain size is small, the lithium ion diffusion path is short, and the lithium ions can be deintercalated in a shorter time, but due to its large specific surface area, there will be more electrolyte-electrode side reaction areas, which is not conducive to the electrochemical performance. If the calcination is more than 900min at 800℃ or above, the material particle size is too large and the particle size distribution is more uneven.

[0042] In order to prevent the material from reacting insufficiently due to too little oxygen or from forming too many oxygen defects in the material due to too much oxygen, the oxygen flow rate in the oxygen atmosphere is controlled to be 58-60 mL / min.

[0043] In order to obtain a dry gel, the drying process is carried out at 200°C to 250°C for 180min to 240min. If the drying temperature is not high enough or the drying time is short, the degree of drying is insufficient, the acetate is not fully volatilized, and the crystallization and structure construction of the material are affected; if the drying temperature is too high or the drying time is long, the precursor structure changes, resulting in the final material may not have a good layered structure.

[0044] The high-nickel ternary oxide material prepared as above is used to prepare the positive electrode material of lithium-ion battery, specifically: the high-nickel ternary metal oxide material, the conductive agent and the binder are mixed in a mass ratio of 7 to 8:1 to 2:1, and then N-methylpyrrolidone is added to obtain a slurry, and an aluminum foil is used as a substrate, and the slurry is evenly coated on the surface of the substrate, and the positive electrode sheet of the lithium-ion battery is obtained after drying; the conductive agent is conductive carbon black, carbon nanotubes or graphene, and the binder is polyvinylidene fluoride or carboxymethyl cellulose.

[0045] The technical effects of the present invention are described in detail below through specific embodiments and comparative examples.

[0046] Example 1

[0047] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0048] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0049] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 5, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a forced air drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0050] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 5h to obtain a precursor.

[0051] S4, heating the precursor at 750° C. for 15 h in an oxygen atmosphere with a flow rate of 60 mL / min to obtain a high-nickel ternary metal oxide material.

[0052] Example 2

[0053] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0054] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0055] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 5, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a forced air drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0056] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 3h to obtain a precursor.

[0057] S4, heating the precursor at 800° C. for 10 h in an oxygen atmosphere with a flow rate of 60 mL / min to obtain a high-nickel ternary metal oxide material.

[0058] Example 3

[0059] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0060] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water; stir evenly to obtain a citric acid solution.

[0061] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 5, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a blast drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0062] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 3h to obtain a precursor.

[0063] S4, heating the precursor at 700° C. for 10 h in an oxygen atmosphere with a flow rate of 60 mL / min to obtain a high-nickel ternary metal oxide material.

[0064] Example 4

[0065] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0066] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0067] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 4, use a constant temperature magnetic stirrer, heat and stir the solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a blast drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0068] S3, crushing the dry gel and placing it in a porcelain boat muffle furnace, and keeping it at 500° C. for 3 h to obtain a precursor.

[0069] S4, heating the precursor at 750° C. for 10 h in an oxygen atmosphere with a flow rate of 58 mL / min to obtain a high-nickel ternary metal oxide material.

[0070] Example 5

[0071] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0072] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0073] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 6, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a forced air drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0074] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 4h to obtain a precursor.

[0075] S4, heating the precursor at 750° C. for 12 h in an oxygen atmosphere with a flow rate of 60 mL / min to obtain a high-nickel ternary metal oxide material.

[0076] Example 6

[0077] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0078] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0079] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 9, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a blast drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0080] S3, crush the dry gel and put it into a porcelain boat muffle furnace, and keep it at 480°C for 3.5h to obtain a precursor.

[0081] S4, heating the precursor at 700° C. for 13 h in an oxygen atmosphere with a flow rate of 60 mL / min to obtain a high-nickel ternary metal oxide material.

[0082] In order to further illustrate the technical effect of the present invention, the present invention also sets a comparative example, which is as follows:

[0083] Comparative Example 1

[0084] Compared with Example 1, the difference is that the oxygen atmosphere is adjusted to an air atmosphere.

[0085] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0086] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water; stir evenly to obtain a citric acid solution.

[0087] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 5, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a blast drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0088] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 5h to obtain a precursor.

[0089] S4, heating the precursor at 750° C. for 15 hours under air atmosphere to obtain a high-nickel ternary metal oxide material.

[0090] Comparative Example 2

[0091] Compared with Example 1, the difference is that the flow rate of the oxygen atmosphere is increased from 60 mL / min to 100 mL / min.

[0092] A method for preparing a high-nickel ternary metal oxide material comprises the following steps:

[0093] S1, dissolve 1.6g nickel acetate, 0.2339g cobalt nitrate, 0.1969g manganese acetate, and 0.8609g lithium acetate in deionized water to obtain a metal salt solution; dissolve 3.4623g citric acid in deionized water, stir evenly, and obtain a citric acid solution.

[0094] S2, slowly drop the citric acid solution into the metal salt solution, stir evenly to obtain a mixed solution, drop ammonia water into the mixed solution to adjust the pH value to 5, use a constant temperature magnetic stirrer, heat the stirred solution in a water bath at 80°C until a wet gel is obtained, place the wet gel in a forced air drying oven, and heat at 200°C for 240 minutes to obtain a dry gel.

[0095] S3, crushing the dry gel and placing it into a porcelain boat muffle furnace, and keeping it at 480°C for 5h to obtain a precursor.

[0096] S4, heating the precursor at 750° C. for 15 h in an oxygen atmosphere with a flow rate of 100 mL / min to obtain a high-nickel ternary metal oxide material.

[0097] Examples 1 to 6 of the present invention all produce high-nickel ternary metal oxide materials with high charge-discharge specific capacity and good capacity retention rate. The high-nickel ternary metal oxide materials of Examples 1 to 3 are used as examples for research. The specific research methods and results are as follows:

[0098] Figure 1 and Figure 2 The results show that the present invention successfully prepared a high-nickel ternary metal oxide material, and the molar ratio of transition metals nickel, cobalt and manganese was 8:1:1.

[0099] Figure 3 to Figure 5 This is the morphology of high nickel ternary metal oxide. Figure 3 to Figure 5 The morphology and structure of high nickel ternary metal oxide materials at calcination temperatures of 700℃, 750℃ and 800℃ respectively. It can be seen that the particle size of NCM811 after calcination at 750℃ is the most moderate.

[0100] Figure 7 The results of the high nickel ternary metal oxide materials calcined at different temperatures at a current density of 200 mAh g -1 The discharge performance diagram shows that the initial discharge capacity of the material calcined at 750 °C is 204.43 mAh g -1 , the specific capacity is significantly improved compared with 700℃ and 800℃.

[0101] Figure 8 The results show that the nickel-rich ternary metal oxide materials can be heated to 200 mAh g under different calcination atmospheres and different oxygen flow rates. -1 The discharge performance diagram shows that the initial discharge capacity of the material calcined at 750 °C is 204.43 mAh g -1 , compared with the calcination in comparative example 1 (air atmosphere) and comparative example 2 (oxygen flow rate of 100 mL / min), the specific capacity is significantly improved.

[0102] In summary, the present invention controls the morphology of the material by controlling the reaction solvent, reaction temperature, reaction pH used in the gel sol reaction process, the reaction temperature and reaction time during the calcination process, and the particle size of the material is controlled within an appropriate range. On the one hand, lithium ions can be deintercalated in a shorter time, and on the other hand, the appropriate particle size reduces the side reactions between the electrolyte and the electrode, thereby improving the lithium storage performance.

[0103] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a high-nickel ternary oxide material, characterized in that: The following steps are involved: Using citric acid as a chelating agent, adding a mixed aqueous solution containing soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to the aqueous solution, mixing, adjusting the pH value to 4-9, stirring at 75-80° C. to combine the transition metal nickel ions, cobalt ions, manganese ions and lithium ions to form a chelate, and drying to obtain a xerogel; The dry gel is crushed, and pre-calcined at 480-500° C. in an air atmosphere to decompose the acetate in the dry gel to obtain a precursor; The precursor is heated to 700-800° C. and calcined in an oxygen atmosphere, so that the precursor gradually forms a layered structure and the crystal particles of the precursor are enlarged, thereby obtaining a high-nickel ternary oxide material.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the soluble transition metal nickel salt, cobalt salt, manganese salt to the soluble lithium salt is 8:1:1:10.

5.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the sum of the soluble transition metal nickel salt, cobalt salt, manganese salt and soluble lithium salt to citric acid is 1:

1.

4. The preparation method according to claim 1, characterized in that: The oxygen flow rate in the oxygen atmosphere is 58-60 mL / min.

5. The preparation method according to claim 1, characterized in that: The pre-calcination time is 180 min to 300 min.

6. The preparation method according to claim 1, characterized in that: The calcination time is 600 min to 900 min.

7. A high-nickel ternary oxide material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the high-nickel ternary oxide material according to claim 7 in preparing a positive electrode material for a lithium-ion battery, characterized in that: A high-nickel ternary metal oxide material, a conductive agent and a binder are mixed in a mass ratio of 7 to 8:1 to 2:1, and N-methylpyrrolidone is added to obtain a slurry. The slurry is evenly coated on the surface of an aluminum foil as a substrate, and a positive electrode sheet of a lithium-ion battery is obtained after drying.

9. The use according to claim 8, characterized in that: The conductive agent is conductive carbon black, carbon nanotube or graphene, and the binder is polyvinylidene fluoride or carboxymethyl cellulose.