Modification method of spinel high-entropy oxide (Fe0. 2Co0. 2Ni0. 2Cr0. 2Mn0. 2) 3O4

By surface modification and bulk doping of spinel high-entropy oxides, modified spinel high-entropy oxides with surface coatings of rock salt-type lithium titanate and amorphous carbon were prepared, solving the problem of low initial lithium insertion/extraction efficiency and achieving high-efficiency electrochemical performance.

CN118929790APending Publication Date: 2024-11-12RES INST OF CHEM DEFENSE PLA ACAD OF MILITARY SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411216161.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The low reversible efficiency of the first lithium insertion/extraction of spinel-type high-entropy oxides has become a bottleneck for their practical application.

Method used

A modification method was developed to prepare oxide particles with a size of 0.1-1 micrometers by employing surface modification and bulk doping strategies. The particles were coated with a composite layer of rock-salt type lithium titanate and amorphous carbon, and titanium was uniformly doped into the bulk phase of the particles.

Benefits of technology

It significantly improved the initial coulombic efficiency to 72.8% and maintained a reversible specific capacity of over 1000 mAh/g after 800 cycles at a current density of 0.5 A/g, demonstrating excellent structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929790A_ABST
    Figure CN118929790A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of electrochemical energy storage materials, and particularly relates to a modification method of a spinel high-entropy oxide (Fe < 0.2 > Co < 0.2 > Ni < 0.2 > Cr < 0.2 > Mn < 0.2 >) 3O4. According to the method, firstly, (Fe0. 2Co0. 2Ni0. 2Cr0. 2Mn0. 2) 3O4 is prepared from a metal oxide precursor through a high-temperature solid-phase method, then the surface of the (Fe0. 2Co0. 2Ni0. 2Cr0. 2Mn0. 2) 3O4 is coated with lithium titanate and amorphous carbon through a solution method, and meanwhile, a bulk phase is uniformly doped with a titanium element. The prepared modified artificial graphite has the structural characteristics that (1) the particle size of the oxide is 0.1-1 micron; (2) a composite coating layer consisting of rock salt type lithium titanate and amorphous carbon is arranged on the surface of the oxide; (3) the thickness of the coating layer is 2-5 nanometers; and (4) the titanium element is uniformly doped in the oxide particle body phase. According to a button cell test, the first coulombic efficiency of the synthesized modified spinel high-entropy oxide (Fe0. 2Co0. 2Ni0. 2Cr0. 2Mn0. 2) 3O4 under the current density of 0.1 A / g is 72.8% and is remarkably higher than the average value of 55%-62% reported in the literature, meanwhile, the reversible specific capacity of over 1,000 mAh / g is still achieved after circulation is conducted for 800 times under the current density of 0.5 A / g, and excellent structural stability is shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical energy storage materials, and specifically relates to a spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method. Background Art

[0002] As a highly efficient energy storage and conversion device, lithium-ion battery (LIB) has many advantages such as high energy density, stable voltage, high output power, low self-discharge rate, adaptability to a wide range of operating temperatures, no memory effect and environmental protection, making it the preferred energy storage device for electric vehicles.

[0003] Currently, commercial LIBs generally use graphite as the negative electrode material. Although it has a lower voltage platform, its theoretical specific capacity is only 370 mAh g -1 Silicon-carbon composite anodes and metal lithium anodes can significantly improve the energy density of lithium batteries, but the cycle life of silicon-carbon composite anodes is still far from the full service life requirements of electric vehicles; the SEI film stability, dendrite growth, interface compatibility and other issues of metal lithium are extremely difficult to overcome, which seriously restricts the industrialization process of metal lithium batteries.

[0004] In recent years, a multi-principal transition metal oxide, high entropy oxide (HEO), has begun to be studied and applied in the field of electrochemical energy storage. config )≥1.6R is called a high entropy oxide (Nature Communication, 2015, 6:8485-8492). HEO breaks the design concept of traditional transition metal oxides. On the one hand, due to the high configurational entropy of the system, it is easy to form simple rock salt type, spinel type and relatively complex fluorite or perovskite solid solution structures; on the other hand, the main elements tend to be arranged in a disordered state, and its chemical composition is in a disordered state, resulting in various performances that are different from traditional transition metal oxides. In comparison, HEO with a specific composition has three significant advantages: (1) Due to the "high entropy effect", it has good structural stability during the cyclic charge and discharge process; (2) The composition contains a variety of electrochemically active metal elements and has a high specific capacity; (3) The performance can be controlled by changing the type and concentration of the metal component, and it has the characteristics of flexible structural design. Among them, the spinel high entropy oxide has a large theoretical specific capacity (usually >1000mAh g -1 ) and is considered to be one of the new LIB negative electrode materials with great development potential.

[0005] However, the current reversible efficiency of the first lithium deintercalation of spinel high entropy oxides is usually only about 50-60% (Nature Communication, 2018, 9: 3400-3408), which is a key bottleneck hindering its practical application. Commonly used improvement strategies are mainly particle nano-sizing, element doping and surface modification. =Related research literature (Journal of Alloys and Compounds 2019, 777: 767-774; Chemical Engineering Journal, 2022, 5: 430-435; Small, 2022, 18: 2200524-2200534) shows that although the improvement strategies of particle nano-sizing and element doping can improve the reversible specific capacity of high entropy oxides, their first coulombic efficiency has hardly changed. This shows that it is difficult to significantly improve the first coulombic efficiency of high entropy oxide negative electrode materials with a single morphology and structure improvement strategy.

[0006] Therefore, it is necessary to develop a modification method for spinel high entropy oxides to overcome the problem of low first coulombic efficiency of high entropy oxide negative electrode materials. Summary of the invention

[0007] The purpose of the present invention is to design a material modification method based on surface modification and bulk doping strategies in order to improve the first coulombic efficiency of spinel high entropy oxide negative electrode materials.

[0008] The modified spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 has the following structural characteristics: (1) The oxide particle size is 0.1-1 micrometers; (2) The oxide surface is a composite coating composed of rock salt type lithium titanate and amorphous carbon; (3) The coating thickness is 2-5 nanometers; (4) The oxide particle bulk phase is uniformly doped with titanium.

[0009] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0010] In a first aspect, the present invention provides a spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, specifically comprising the following steps:

[0011] (1) weighing metal oxides of Fe, Co, Ni, Cr, and Mn metal elements in equal molar proportions as synthetic raw materials, and grinding them thoroughly to obtain a mixed powder;

[0012] (2) placing the mixed powder in a tube furnace, heating the temperature from room temperature to 850°C to 1200°C at a rate of 3°C / min to 9°C / min in an air environment, maintaining the temperature for 5 to 24 hours, and then cooling naturally to room temperature to obtain (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide;

[0013] (3) weighing a lithium source and a titanium source as raw materials for preparing a lithium titanate coating layer according to a molar ratio of lithium to titanium of 1:0.8 to 0.9, and weighing and mixing the lithium titanate and the spinel high entropy oxide according to a measured mass ratio of 0.5 to 10:100, and then adding an alcohol solution to prepare a slurry; wherein the mass ratio of the total mass of the lithium source, the titanium source and the spinel high entropy oxide to the alcohol solution is 5 to 20:100;

[0014] (4) grinding the slurry to remove the solvent, washing with alcohol solution until clean, collecting the solid powder after removing the solvent, placing it in an oven at 60° C. to 80° C. to dry it completely, and obtaining a spinel high entropy oxide powder with a surface coated with a lithium titanate precursor;

[0015] (5) placing the powder obtained in step (4) in a tube furnace, heating the temperature from room temperature to 850°C to 1200°C at a rate of 3°C / min to 9°C / min under an inert gas environment, maintaining the temperature for 5 to 24 hours, and then cooling naturally to room temperature to obtain the modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide powder.

[0016] Preferably, the lithium source is lithium hydroxide, lithium carbonate or lithium acetate.

[0017] Preferably, the titanium source is tetrabutyl titanate, isopropyl titanate, n-propyl titanate, ethyl titanate, titanium sulfate, titanium chloride or orthotitanic acid.

[0018] Preferably, the metal oxides in step (1) are ferric oxide, cobalt oxide, nickel oxide, chromium oxide and manganese dioxide.

[0019] Preferably, the grinding method of the metal oxide in step (1) is: placing it in a planetary ball mill and ball milling it at a rotation speed of 200 to 450 rpm for 2 to 10 hours.

[0020] Preferably, in the step (4), the slurry is ball-milled at a rotation speed of 200 rpm to 800 rpm for 5 to 10 hours, and then the solvent is removed by vacuum filtration.

[0021] Preferably, the alcohol solution in step (3) and step (4) is an ethanol solution, and the inert gas in step (5) is argon.

[0022] In a second aspect, the present invention provides a modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide.

[0023] Preferably, the modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 The main particle size of the 3O4 spinel high entropy oxide powder is 0.1-1 micron, and the surface is coated with a composite layer composed of rock salt type lithium titanate and amorphous carbon. The coating layer thickness is 2-5nm, and titanium is uniformly doped in the oxide particle phase.

[0024] In a third aspect, the present invention provides a modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide as negative electrode for lithium batteries.

[0025] Beneficial effects achieved by the present invention:

[0026] (1) The surface of the oxide particles is coated with rock salt type lithium titanate and amorphous carbon at the same time; (2) The lithium ion conductor phase in the coating layer is rock salt type lithium titanate, which not only improves the interfacial lithium ion transmission capacity but also inhibits the side reactions of the electrolyte; (3) The electronic conductor phase in the coating layer is amorphous carbon, which can improve the surface electronic conductivity and reduce the polarization effect of lithium insertion and extraction reactions; (4) The bulk phase of the oxide particles is uniformly doped with titanium to improve the cycle stability; (5) The synthesis method is simple and highly repeatable.

[0027] The synthesized modified spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2)3O4 has a first coulombic efficiency of 72.8% at a current density of 0.1A / g, which is significantly higher than the average value of 55%-62% reported in the literature. At the same time, it still has a reversible specific capacity of more than 1000mAh / g after 800 cycles at a current density of 0.5A / g, showing excellent structural stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The SEM image of the modified spinel high entropy oxide prepared by the method of the present invention is

[0029] Figure 2 The metal element distribution diagram of the cross section of the modified spinel high entropy oxide prepared by the method of the present invention is

[0030] Figure 3 TEM image of the modified spinel high entropy oxide prepared by the method of the present invention

[0031] (a) 5nm size; (b) 10nm size;

[0032] Figure 4 The XRD pattern of the modified spinel high entropy oxide prepared by the method of the present invention is

[0033] In the figure: the ordinate is the diffraction intensity, and the abscissa is the diffraction angle 2θ, and the unit is °.

[0034] Figure 5 The first charge and discharge curve of the modified spinel high entropy oxide prepared by the method of the present invention is

[0035] In the figure: the vertical axis is voltage, the unit is V, and the horizontal axis is specific capacity, the unit is mAh / g.

[0036] Figure 6 The modified spinel high entropy oxide prepared by the method of the present invention was cycled 800 times at 0.5A / g.

[0037] In the figure: the vertical axis is the specific capacity, the unit is mAh / g, and the horizontal axis is the number of cycles, the unit is times.

[0038] Figure 7 This is the first charge and discharge curve of the unmodified spinel high entropy oxide negative electrode material of Comparative Example 1;

[0039] Figure 8 This is the long cycle performance diagram of the unmodified spinel high entropy oxide negative electrode material of Comparative Example 1. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0042] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0043] Example 1

[0044] (1) weighing 1.6 g of ferric oxide, 2.4 g of cobalt oxide, 0.75 g of nickel oxide, 1.52 g of chromium oxide, and 0.87 g of manganese dioxide as synthetic raw materials, placing them in a planetary ball mill, and ball milling them at a speed of 300 rpm for 3 hours to obtain a mixed powder;

[0045] (2) The mixed powder was placed in a tube furnace, heated from room temperature to 850°C at a rate of 6°C / min in an air environment, kept at this temperature for 5 hours, and then naturally cooled to room temperature to obtain (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide;

[0046] (3) Take 2g of the prepared (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide is dispersed in 40 mL of anhydrous ethanol to obtain suspension A, 0.74 g of tetrabutyl titanate is dissolved in 20 mL of anhydrous ethanol to obtain sol B, and then sol B is added dropwise to suspension A, after reacting for 1 hour, 0.12 g of anhydrous lithium acetate is added, and the mixed system is ball-milled at a rotation speed of 350 rpm for 6 hours to obtain a suspension slurry of modified spinel high entropy oxide precursor;

[0047] (4) After ball milling the suspension slurry at 350 rpm for 6 hours, vacuum filtration was used to remove the solvent, and the solid powder was collected and dried in an oven at 60° C. to 80° C. to obtain a spinel high entropy oxide powder with a surface coated with a lithium titanate precursor;

[0048] (5) The dried powder was placed in a tube furnace, heated from room temperature to 850°C at a rate of 6°C / min in an air environment, kept at this temperature for 5 hours, and then naturally cooled to room temperature to obtain the modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide powder;

[0049] (6) The prepared modified spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 negative electrode material, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 7:2:1, and slurry was prepared with nitrogen methyl pyrrolidone and coated on copper foil. After drying at 80°C for 24 hours, the slurry was cut into discs with a diameter of 16 mm. The cut discs were further dried in a vacuum at 120°C for 4 hours, and then moved into an argon glove box to be assembled into button batteries with metal lithium sheets and 1M LiPF6 EC / DEC (volume ratio 1:1) electrolyte. The batteries were then tested using LANHE CT3004A in the current range of 0.1A / g-0.5A / g.

[0050] (7) The morphology of the prepared modified high entropy oxide is shown in the attached Figure 1 -Attached Figure 3 、Phase analysis see attached Figure 4 , proving that its surface is a composite coating composed of rock salt type lithium titanate and amorphous carbon, and that the particle phase is uniformly doped with titanium

[0051] (8) The first charge-discharge curve and cycle life of the prepared modified high entropy oxide are shown in the attached Figure 5 -Attached Figure 6 , showing that the first coulombic efficiency at 0.1A / g is 72.8%, and the reversible specific capacity reaches 1123mAh / g after 800 cycles at 0.5A / g.

[0052] Comparative Example 1

[0053] (1) The unmodified spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2)3O4 negative electrode material, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 7:2:1, and slurry was prepared with nitrogen methyl pyrrolidone and coated on copper foil. After drying at 80°C for 24 hours, the slurry was cut into discs with a diameter of 16 mm. The cut discs were further dried in a vacuum at 120°C for 4 hours, and then moved into an argon glove box to be assembled into button batteries with metal lithium sheets and 1M LiPF6 EC / DEC (volume ratio 1:1) electrolyte. The batteries were then tested using LANHE CT3004A in the current range of 0.1A / g-0.5A / g.

[0054] (2) The first charge and discharge curves of the unmodified spinel high entropy oxide negative electrode material at 0.1A / g and the long cycle performance at 0.5A / g are shown in the figure below. The data show that its first coulombic efficiency is only 63.7%, and its reversible specific capacity gradually decays after the 600th cycle, and drops to about 600mAh / g after the 800th cycle.

[0055] Based on the experimental data of Example 1 and Comparative Example 1, the modified spinel high entropy oxide negative electrode material prepared by the present method has excellent cycle stability and high first coulombic efficiency, reaching the advanced level of similar materials.

Claims

1. A spinel high entropy oxide (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The specific steps include: (1) weighing metal oxides of Fe, Co, Ni, Cr, and Mn metal elements in equal molar proportions as synthetic raw materials, and grinding them thoroughly to obtain a mixed powder; (2) The mixed powder is heated from room temperature to 850°C to 1200°C at a rate of 3°C / min to 9°C / min in an air environment, kept at this temperature for 5 to 24 hours, and then cooled naturally to room temperature to obtain (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide; (3) weighing a lithium source and a titanium source as raw materials for preparing a lithium titanate coating layer according to a molar ratio of lithium to titanium of 1:0.8 to 0.9, and weighing and mixing the lithium titanate and the spinel high entropy oxide according to a measured mass ratio of 0.5 to 10:100, and then adding an alcohol solution to prepare a slurry; wherein the mass ratio of the total mass of the lithium source, the titanium source and the spinel high entropy oxide to the alcohol solution is 5 to 20:100; (4) grinding the slurry to remove the solvent, washing with alcohol solution until clean, collecting the solid powder after removing the solvent, placing it in an oven at 60° C. to 80° C. to dry it completely, and obtaining a spinel high entropy oxide powder with a surface coated with a lithium titanate precursor; (5) The powder obtained in step (4) is heated from room temperature to 850°C to 1200°C at a rate of 3°C / min to 9°C / min under an inert gas environment, maintained at this temperature for 5 to 24 hours, and then naturally cooled to room temperature to obtain a modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide powder.

2. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The lithium source is lithium hydroxide, lithium carbonate or lithium acetate.

3. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The titanium source is tetrabutyl titanate, isopropyl titanate, n-propyl titanate, ethyl titanate, titanium sulfate, titanium chloride or orthotitanic acid.

4. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The metal oxides in step (1) are respectively ferric oxide, cobalt oxide, nickel oxide, chromium oxide and manganese dioxide.

5. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The grinding method of the metal oxide in step (1) is: placing it in a planetary ball mill and ball milling it at a rotation speed of 200 to 450 rpm for 2 to 10 hours.

6. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, In the step (4), the slurry is ball-milled at a rotation speed of 200 rpm to 800 rpm for 5 to 10 hours, and then the solvent is removed by vacuum filtration.

7. The spinel high entropy oxide (Fe) according to claim 1 0.2 Co 0.2Ni 0.2 Cr 0.2 Mn 0.2 )3O4 modification method, characterized in that, The alcohol solution in step (3) and step (4) is ethanol solution, and the inert gas in step (5) is argon.

8. A modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide.

9. The modified (Fe) according to claim 8 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide, characterized in that The modified (Fe 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 The main particle size of the 3O4 spinel high entropy oxide powder is 0.1-1 micron, and the surface is coated with a composite layer composed of rock salt type lithium titanate and amorphous carbon. The coating layer thickness is 2-5nm, and titanium is uniformly doped in the oxide particle phase.

10. A modified (Fe) according to claim 8 or 9 0.2 Co 0.2 Ni 0.2 Cr 0.2 Mn 0.2 )3O4 spinel high entropy oxide as negative electrode for lithium batteries.

Citation Information

Cited By

  • Sludge-based high-entropy oxide catalyst and preparation method thereof

    CN120243048A

  • Chromium-site high-entropy chromium lithium titanate material as well as preparation method and application thereof

    CN121342087A