Two-dimensional stepped nickel oxide nanosheet and preparation method thereof

Through potassium iodide-assisted atmospheric chemical vapor deposition method, the problem of difficulty in preparing large-size high-density two-dimensional nickel oxide nanosheets in the prior art is solved, especially the step-like structure, and direct growth on the silica substrate is achieved , provides suitable catalytic activity research conditions.

CN118929791APending Publication Date: 2024-11-12SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410508731.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult to prepare large-size and high-density two-dimensional nickel oxide nanosheets, especially step-like structures, and it is difficult to directly prepare two-dimensional oxide nanosheets on silica substrates.

Method used

Using potassium iodide-assisted atmospheric chemical vapor deposition method, a mixture of nickel source and potassium iodide was used to react at 500-800°C for 1 to 30 minutes to prepare large-size high-density two-dimensional step-shaped nickel oxide nanosheets, and the amount of potassium iodide was adjusted. and growth time to regulate the density and size of nanosheets.

Benefits of technology

Successfully synthesized a large-size high-density two-dimensional step-shaped nickel oxide nanosheet array with a thickness of nearly a single layer and adjustable size, which helps in the study of growth kinetics and catalytic activity of two-dimensional materials, and can be directly on the silica substrate. Grow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929791A_ABST
    Figure CN118929791A_ABST
Patent Text Reader

Abstract

The invention discloses a two-dimensional stepped nickel oxide nanosheet and a preparation method thereof. The preparation method comprises the following steps: adopting a chemical vapor deposition method, taking a mixture of a nickel source and potassium iodide as a growth precursor, and reacting at 500-800 DEG C for 1-30 minutes to prepare the two-dimensional stepped nickel oxide nanosheet. The large-size high-density two-dimensional ladder-shaped nickel oxide nanosheet array is synthesized by adopting a potassium iodide assisted normal-pressure chemical vapor deposition preparation method, the synthesized nickel oxide is a two-dimensional ladder-shaped nanosheet, and the ladder-shaped structure of the two-dimensional ladder-shaped nanosheet is beneficial to research on two-dimensional material growth kinetics and catalytic activity related to exposed crystal faces; and the growth can reach a single-layer thickness, and the size is adjustable in a range from several microns to dozens of microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a nickel oxide nanosheet, in particular to a two-dimensional stepped nickel oxide nanosheet and a method for preparing the same, and belongs to the field of nano science and technology. Background Art

[0002] Nickel oxide (NiO) is a native p-type semiconductor with high transparency. It is an important inorganic material with a variety of uses, such as electrochemical electrodes, heterogeneous catalysis, hole transport layers, and electrochromic layers. At the same time, bulk NiO is an antiferromagnetic material. Previous studies have found that when the size of NiO is reduced to a two-dimensional layer, it is possible to exhibit ferromagnetism (Angew.Chem.Int.Ed.2021, 60, 25020-25027). NiO film also has piezoelectric effect and photovoltaic behavior (Adv.Sci.2023, 10, 2304637), which is also an excellent heterogeneous catalytic material (Chemical EngineeringJournal 436 (2022) 135041).

[0003] The main methods for preparing two-dimensional nickel oxide nanosheets at present are hydrothermal method, magnetron sputtering, electron beam evaporation and atomic layer deposition. However, most of the materials obtained by these methods are bulk materials or nanoparticles. The prepared two-dimensional nickel oxide nanosheets are small in size and the steps are cumbersome. It is difficult to obtain large-sized and high-density nickel oxide single crystal nanosheets. It is also difficult to obtain nickel oxide nanosheets with stepped growth, and it is also difficult to directly prepare two-dimensional oxide nanosheets on a silicon dioxide substrate. There is no report on the preparation of two-dimensional nickel oxide nanosheets by a bottom-up chemical vapor deposition method. Summary of the invention

[0004] The main purpose of the present invention is to provide a two-dimensional stepped nickel oxide nanosheet and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] An embodiment of the present invention provides a method for preparing a two-dimensional stepped nickel oxide nanosheet, which comprises: adopting a chemical vapor deposition method, using a mixture of a nickel source and potassium iodide as a growth precursor, reacting at 500 to 800° C. for 1 to 30 minutes, to obtain a two-dimensional stepped nickel oxide nanosheet.

[0007] In some preferred embodiments, the preparation method includes: using chemical vapor deposition, placing a growth precursor and a growth substrate in a reaction chamber of a chemical vapor deposition device, and depositing two-dimensional stepped nickel oxide nanosheets prepared by the reaction on the surface of the growth substrate.

[0008] In some preferred embodiments, the preparation method comprises: raising the temperature in the reaction chamber to 500-800° C. at a heating rate of 10-50° C. / min.

[0009] The embodiment of the present invention further provides a two-dimensional stepped nickel oxide nanosheet, which is prepared by the aforementioned preparation method.

[0010] Compared with the traditional synthesis method, the beneficial effects of the present invention are:

[0011] The present invention adopts a potassium iodide-assisted atmospheric pressure chemical vapor deposition preparation method to synthesize a large-size and high-density two-dimensional stepped nickel oxide nanosheet array. The synthesized nickel oxide is a two-dimensional stepped nanosheet, and its stepped structure is helpful for the study of the growth dynamics of two-dimensional materials and the catalytic activity related to the exposed crystal surface. It can grow to a single layer thickness and has an adjustable size within the range of several microns to tens of microns. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1 It is a schematic diagram of a process for preparing two-dimensional stepped nickel oxide nanosheets by atmospheric pressure chemical vapor deposition (APCVD) in a typical embodiment of the present invention;

[0014] Figure 2a-2c is an optical microscope image of the two-dimensional stepped nickel oxide nanosheets prepared in Example 1 of the present invention;

[0015] Figure 3a-Figure 3b is an atomic force microscope (AFM) image of the two-dimensional stepped nickel oxide nanosheet prepared in Example 1 of the present invention;

[0016] Figure 4a-4b is an atomic force microscope (AFM) image of the two-dimensional stepped nickel oxide nanosheets prepared in Example 2 of the present invention on a silicon oxide substrate;

[0017] Figure 5 is an EDS element spectrum of the two-dimensional stepped nickel oxide nanosheets prepared in Example 1 of the present invention;

[0018] Figure 6 is an atomic force microscope (AFM) image of the two-dimensional flat nickel oxide nanosheet prepared in Comparative Example 2;

[0019] Figure 7is a height diagram of nickel oxide nanosheets along the white line in Comparative Example 2;

[0020] Figure 8 is an optical microscope image of the nanosheet prepared in Comparative Example 3;

[0021] Fig. 9 is an optical microscope image of the nanosheet prepared in Comparative Example 4;

[0022] Fig.10 is an optical microscope image of the nanosheet prepared in Comparative Example 5;

[0023] Fig.11 This is an optical microscope image of the nanosheets prepared in Comparative Example 6. DETAILED DESCRIPTION

[0024] In view of the shortcomings of the prior art, the inventors of this case proposed the technical concept of the present invention after long-term research. For the first time, they used potassium iodide-assisted atmospheric pressure chemical vapor deposition (APCVD) to synthesize large-scale and high-density two-dimensional stepped nickel oxide nanosheet arrays, whose thickness is close to that of a single layer of nickel oxide, and the size can be adjusted from a few microns to tens of microns.

[0025] The technical solution, its implementation process and principle will be further explained as follows.

[0026] As one aspect of the technical solution of the present invention, a method for preparing a two-dimensional stepped nickel oxide nanosheet involves: using atmospheric pressure chemical vapor deposition (APCVD), using a mixture of a nickel source and potassium iodide (KI) as a growth precursor, reacting at 500-800°C for 1-30 minutes, to obtain a two-dimensional stepped nickel oxide nanosheet.

[0027] Compared with sodium chloride, the preparation mechanism of the present invention is that the melting point of potassium iodide is 618°C, and the melting point of sodium chloride is 801°C. Potassium iodide is more likely to participate in the reaction in the temperature range of 500-800°C, and the reaction temperature is reduced. The addition of potassium iodide affects the nucleation density and the formation of step-like nanosheets, and can provide a more intense growth kinetic environment, thereby obtaining two-dimensional nickel oxide nanosheets with step-like growth. Among them, the growth density and step-like structure of the two-dimensional nickel oxide nanosheets can be adjusted by adjusting the amount of potassium iodide added; and the size of the nanosheets can be adjusted by adjusting the growth time.

[0028] In some more specific implementation cases, the preparation method includes: using chemical vapor deposition, placing a growth precursor and a growth substrate in a reaction chamber of a chemical vapor deposition device, and depositing the two-dimensional stepped nickel oxide nanosheets prepared by the reaction on the surface of the growth substrate.

[0029] In some more specific implementation cases, the preparation method includes: placing a growth precursor in a reaction chamber of a chemical vapor deposition device, heating to 500-800°C, and allowing the growth precursor to be deposited on the surface of a growth substrate under the action of a carrier gas. The growth temperature used in the present invention is a key influencing factor, and the growth temperature can be 500-800°C.

[0030] In the present invention, the growth time is also a key influencing factor, which can control the size of the obtained nickel oxide nanosheets. The commonly used growth time is 1 to 30 minutes.

[0031] Further, the nickel source includes nickel chloride (NiCl2), nickel chloride hexahydrate (NiCl2·6H2O), etc., but is not limited thereto.

[0032] Furthermore, the molar ratio of the nickel source to potassium iodide is 1:0.02 to 1:0.05. In the present invention, the type of growth raw material precursor cannot be changed at will, otherwise the two-dimensional stepped nickel oxide nanosheets cannot be grown. And the added potassium iodide will affect the nucleation density of the nanosheets. Specifically, the addition of potassium iodide can increase the nucleation density and the growth of stepped structure nanosheets, and can be grown on a silicon dioxide substrate. Without adding potassium iodide, nanosheets can also be grown using only nickel chloride or nickel chloride hexahydrate, but a stepped structure cannot be grown.

[0033] In some implementation cases, the growth substrate can be a freshly dissociated fluorphlogopite sheet, which can be placed obliquely or flat about 3 mm above the precursor. The present invention uses a potassium iodide-assisted chemical vapor deposition method to prepare stepped nickel oxide nanosheets on mica sheets, and can also prepare nickel oxide nanosheets on silicon dioxide substrates, and the size and density are adjustable, which helps to understand the growth mechanism of two-dimensional oxides. At the same time, nickel oxide nanosheets can be grown directly on silicon dioxide substrates, which is beneficial to the subsequent device preparation and physical property research.

[0034] In some implementation cases, the growth substrate is disposed upside down on the growth precursor.

[0035] Furthermore, during the first step of the growth process, the growth substrate may be placed in a tilted manner or in a horizontal manner and inverted.

[0036] In some implementation cases, the growth precursor is disposed between at least two growth substrates for spatially confined growth, or the growth precursor is disposed in the central region of the reaction chamber. More specifically, the growth precursor can be placed not only directly in a quartz boat, but also sandwiched between two freshly dissociated mica sheets for spatially confined growth, and two-dimensional stepped nickel oxide nanosheets can also be obtained.

[0037] In some more preferred implementation cases, the preparation method comprises: raising the temperature in the reaction chamber to 500-800°C at a heating rate of 10-50°C / min, preferably 10-30°C / min. In the present invention, the heating rate is an auxiliary influencing factor during the growth of the two-dimensional stepped nickel oxide nanosheets, and 10-50°C / min is the preferred heating rate for growing nanobelts.

[0038] In summary, in the growth process of the present invention, the heating rate can range from 10 to 50°C / min, the growth temperature can range from 500°C to 800°C, the growth time can range from 1min to 30min, and different growth conditions correspond to different sizes and morphologies of two-dimensional stepped nickel oxide nanosheets.

[0039] In some implementation cases, the preparation method includes: before the reaction, introducing a carrier gas with a flow rate of 100 to 300 sccm into the reaction chamber for 5 to 10 minutes to remove the air in the reaction chamber.

[0040] Furthermore, the carrier gas includes an inert gas, such as argon (Ar). The present invention uses Ar as the carrier gas, cleans the quartz pipe before growth, and the flow rate during the growth process is 100-300 sccm.

[0041] Compared with the traditional synthesis method, the growth process of the two-dimensional stepped nickel oxide nanosheets in the present invention uses a normal pressure chemical vapor deposition method and uses Ar as a carrier gas. The entire growth process is relatively simple and has low energy consumption.

[0042] Furthermore, the preparation method further comprises: adjusting the flow rate of the carrier gas to 100-300 sccm, stabilizing for 1-5 minutes, and then heating to 500-800°C.

[0043] In some more specific implementation cases, the preparation method further comprises: after the reaction is completed, the temperature in the reaction chamber is rapidly reduced to room temperature at a rate of 30-50°C / min, thereby obtaining two-dimensional stepped nickel oxide nanosheets. The cooling process adopted by the present invention is rapid cooling, and the quartz tube is directly moved out of the high temperature zone and rapidly reduced to room temperature.

[0044] See also Figure 1As shown, it is a schematic diagram of preparing two-dimensional stepped nickel oxide nanosheets by atmospheric pressure chemical vapor deposition (APCVD) in the present invention. The present invention uses an atmospheric pressure chemical vapor deposition system (Thermo Scientific LBM1100℃Mini-MiteTM single-zone tube furnace), selects nickel chloride (NiCl2, 10-20 mg, Alfa-Aesar) or nickel chloride hexahydrate (NiCl2·6H2O, 10-20 mg, Alfa-Aesar) and potassium iodide (KI, about 2 mg, Alfa-Aesar) as growth precursors (potassium iodide affects the nucleation density and the formation of stepped nanosheets), and mica is used as a growth substrate. Before growth, NiCl2 or NiCl2·6H2O and KI are ground and mixed uniformly according to a molar ratio of 1:0.02 to 1:0.05, and placed in a quartz boat (100mm×10mm×5mm). Then, the freshly dissociated mica sheet is used as a growth substrate, and is inverted on the top of the growth precursor without contacting the growth precursor. The quartz boat with the growth precursor and the growth substrate is placed in the middle of the quartz tube of the tube furnace, and the CVD growth system is closed. Argon (Ar, 99.995%, 300sccm) is passed for cleaning for 10 minutes. After 10 minutes, the Ar flow rate is adjusted from 300sccm to 100sccm, and the tube furnace is heated to 500-800°C at a heating rate of 10-50°C / min, and the temperature is kept for 1-30 minutes. The quartz tube is then pushed out of the high temperature zone and quickly cooled to room temperature, thereby obtaining a two-dimensional stepped nickel oxide nanosheet. If potassium iodide is not added, nanosheets can also be grown using only nickel chloride or nickel chloride hexahydrate. However, the addition of potassium iodide can provide a more intense growth kinetic environment, thereby obtaining a stepped-grown two-dimensional nickel oxide nanosheet.

[0045] As another aspect of the technical solution of the present invention, it also relates to a two-dimensional stepped nickel oxide nanosheet prepared by the aforementioned preparation method, which has a stepped structure.

[0046] Furthermore, compared with the traditional synthesis method, the nickel oxide synthesized by the present invention is a two-dimensional stepped nanosheet array, and the stepped structure is helpful for the study of the growth dynamics of two-dimensional materials and the catalytic activity related to the exposed crystal surface. In addition, its thickness is close to that of a single layer of nickel oxide, with a size of 1 to 50 μm, preferably adjustable within a range of several microns to tens of microns.

[0047] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on it. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or under the conditions recommended by the manufacturer.

[0048] Example 1

[0049] (1) Single-zone tube furnace CVD system: Thermo Scientific LBM1100°C Mini-MiteTM single-zone tube furnace

[0050] (2) Nickel chloride (NiCl2, Alfa-Aesar) and potassium iodide (KI, Alfa-Aesar)

[0051] (3) Growth substrate: freshly dissociated surface of fluorphlogopite mica; quartz boat: 100 mm × 10 mm × 5 mm

[0052] (4) NiCl2 and KI are mixed evenly at a molar ratio of 1:0.02, placed in a quartz boat, and the freshly dissociated mica sheet is placed upside down on top of the precursor, and the quartz boat is placed in the center of the constant temperature area of ​​the tube furnace. Before growth, Ar gas with a flow rate of 300sccm is passed for 10 minutes to clear the residual air in the pipeline. Then the Ar gas flow rate is adjusted from 300sccm to 100sccm and stabilized for 1 minute. Then, the center temperature of the tube furnace is raised to 600℃ at a heating rate of 30℃ / min, and kept warm for 20 minutes. Then, the quartz tube is pushed out of the high temperature zone and quickly cooled to room temperature to obtain a two-dimensional stepped nickel oxide nanosheet.

[0053] The inventors of this case characterized the two-dimensional stepped nickel oxide nanosheets obtained in this example, and the results are as follows:

[0054] See also Figure 2a-2c As shown in FIG. 1 , an optical microscope image of a two-dimensional stepped nickel oxide nanosheet is shown. As can be seen from the image, the size of the nickel oxide nanosheet can reach 10-30 microns. The present invention can adjust the growth density and stepped structure of the two-dimensional nickel oxide nanosheet by adjusting the amount of added KI; and can adjust the size of the nanosheet by adjusting the growth time.

[0055] Figure 3a and Figure 3bThis is an atomic force microscope (AFM) image of a two-dimensional stepped nickel oxide nanosheet. It can be seen from the image that the two-dimensional nickel oxide nanosheet grows in a stepped manner and can reach a single layer of nickel oxide thickness. The two-dimensional stepped nickel oxide nanosheet is helpful for the study of the growth dynamics of two-dimensional materials and the catalytic activity related to the exposed crystal surface. Figure 5 This is the EDS elemental spectrum of two-dimensional stepped nickel oxide nanosheets.

[0056] Example 2

[0057] (1) Single-zone tube furnace CVD system: Thermo Scientific LBM1100°C Mini-MiteTM single-zone tube furnace

[0058] (2) Nickel chloride hexahydrate (NiCl2·6H2O, Alfa-Aesar) and potassium iodide (KI, Alfa-Aesar)

[0059] (3) Growth substrate: silicon dioxide substrate; quartz boat: 100 mm × 10 mm × 5 mm

[0060] (4) NiCl2·6H2O and KI were mixed evenly at a molar ratio of 1:0.02, placed in a quartz boat, the silicon dioxide substrate was placed upside down on top of the precursor, and the quartz boat was placed in the center of the constant temperature area of ​​the tube furnace. Before growth, Ar gas with a flow rate of 300sccm was passed for 10min to clear the residual air in the pipeline. Then the Ar gas flow rate was adjusted from 300sccm to 100sccm and stabilized for 1min. Then, the center temperature of the tube furnace was raised to 500℃ at a heating rate of 10℃ / min, kept warm for 30min, and then the quartz tube was pushed out of the high temperature zone and quickly cooled to room temperature to obtain a two-dimensional stepped nickel oxide nanosheet.

[0061] Figure 4a and Figure 4b This is an optical microscope image of two-dimensional stepped nickel oxide nanosheets on a silicon oxide substrate. It can be seen from the image that the size of the nickel oxide nanosheets can reach 60-70 microns.

[0062] Example 3

[0063] (1) Single-zone tube furnace CVD system: Thermo Scientific LBM1100°C Mini-MiteTM single-zone tube furnace

[0064] (2) Nickel chloride (NiCl2, Alfa-Aesar) and potassium iodide (KI, Alfa-Aesar)

[0065] (3) Growth substrate: freshly dissociated surface of fluorphlogopite mica; quartz boat: 100 mm × 10 mm × 5 mm

[0066] (4) NiCl2 and KI are mixed evenly at a molar ratio of 1:0.02, placed in a quartz boat, and the freshly dissociated mica sheet is placed upside down on top of the precursor, and the quartz boat is placed in the center of the constant temperature area of ​​the tube furnace. Before growth, Ar gas with a flow rate of 300sccm is passed for 10 minutes to clear the residual air in the pipeline. Then the Ar gas flow rate is adjusted from 300sccm to 100sccm and stabilized for 1 minute. Then, the center temperature of the tube furnace is raised to 800℃ at a heating rate of 50℃ / min, and kept warm for 1 minute. Then, the quartz tube is pushed out of the high temperature zone and quickly cooled to room temperature to obtain a two-dimensional stepped nickel oxide nanosheet.

[0067] Example 4

[0068] Compared with Example 1, the difference between this embodiment and Example 1 is that: (4) NiCl2 and KI are mixed evenly at a molar ratio of 1:0.03, placed in a quartz boat, and the freshly dissociated mica sheet is placed upside down on top of the precursor, and the quartz boat is placed in the center of the constant temperature area of ​​the tube furnace. Before growth, Ar gas with a flow rate of 200sccm is passed for 5min to clear the residual air in the pipeline. Then the Ar gas flow rate is adjusted from 200sccm to 100sccm and stabilized for 5min. Then, the center temperature of the tube furnace is raised to 600℃ at a heating rate of 20℃ / min, and kept warm for 15min. Then, the quartz tube is pushed out of the high temperature zone and quickly cooled to room temperature to obtain a two-dimensional stepped nickel oxide nanosheet.

[0069] Example 5

[0070] Compared with Example 1, the difference between this embodiment and Example 1 is that: (4) NiCl2 and KI are mixed evenly at a molar ratio of 1:0.05, placed in a quartz boat, and the freshly dissociated mica sheet is placed upside down on top of the precursor, and the quartz boat is placed in the center of the constant temperature area of ​​the tube furnace. Before growth, Ar gas with a flow rate of 300sccm is passed for 5min to clear the residual air in the pipeline. Then the Ar gas flow rate is adjusted from 300sccm to 200sccm and stabilized for 2min. Then, the center temperature of the tube furnace is raised to 700℃ at a heating rate of 30℃ / min, and kept warm for 10min. Then, the quartz tube is pushed out of the high temperature zone and quickly cooled to room temperature to obtain a two-dimensional stepped nickel oxide nanosheet.

[0071] Comparative Example 1

[0072] Compared with Example 1, this comparative example differs in that potassium iodide is not added.

[0073] The final product, nickel oxide nanosheets, has a flat planar structure and does not have a stepped structure.

[0074] Comparative Example 2

[0075] The difference between this comparative example and Example 1 is that potassium iodide is replaced by sodium chloride.

[0076] The final product, nickel oxide nanosheets, has a flat planar structure without a step-like structure. The atomic force microscope (AFM) image is shown below. Figure 6 The height map of nickel oxide nanosheets along the white line is shown in Figure 7 shown.

[0077] Comparative Example 3

[0078] Compared with Example 1, the difference between this comparative example is that the molar ratio of NiCl2 to KI is 1:0.01, and the final product is very sparse nanosheets, such as Figure 8 shown.

[0079] Comparative Example 4

[0080] Compared with Example 1, the difference between this comparative example is that the molar ratio of NiCl2 to KI is 1:0.08, and the final product is irregularly shaped and dense nanosheets, such as Fig. 9 shown.

[0081] Comparative Example 5

[0082] The difference between this comparative example and Example 1 is that the center temperature of the tube furnace is raised to 400°C, and finally almost no sample nucleation growth occurs. Fig.10 shown.

[0083] Comparative Example 6

[0084] The difference between this comparative example and Example 1 is that the center temperature of the tube furnace is raised to 900°C. The final product morphology is as follows Fig.11 As shown, it is shown that its nucleation is very sparse and very thick.

[0085] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0086] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.

Claims

1. A method for preparing two-dimensional stepped nickel oxide nanosheets, characterized in that: include: The chemical vapor deposition method is adopted, a mixture of a nickel source and potassium iodide is used as a growth precursor, and the reaction is carried out at 500-800° C. for 1-30 minutes to prepare a two-dimensional stepped nickel oxide nanosheet.

2. The preparation method according to claim 1, characterized in that: include: By adopting the chemical vapor deposition method, a growth precursor and a growth substrate are placed in a reaction chamber of a chemical vapor deposition device, and two-dimensional stepped nickel oxide nanosheets prepared by the reaction are deposited on the surface of the growth substrate.

3. The preparation method according to claim 2, characterized in that: The method comprises: placing a growth precursor in a reaction chamber of a chemical vapor deposition device, heating the growth precursor to 500-800° C., and allowing the growth precursor to be deposited on the surface of a growth substrate under the action of a carrier gas.

4. The preparation method according to claim 1, characterized in that: The nickel source includes nickel chloride and / or nickel chloride hexahydrate; and / or the molar ratio of the nickel source to potassium iodide is 1:0.02 to 1:0.

05.

5. The preparation method according to claim 2, characterized in that: The growth substrate comprises any one of a mica sheet and a silicon dioxide substrate; and / or the growth substrate is arranged inverted above the growth precursor; preferably, the growth substrate is arranged tilted or placed horizontally; preferably, the growth precursor is arranged between at least two growth substrates for spatially confined growth; preferably, the growth precursor is arranged in the central area of ​​the reaction chamber.

6. The preparation method according to claim 3, characterized in that: include: The temperature in the reaction chamber is raised to 500-800° C. at a heating rate of 10-50° C. / min, preferably 10-30° C. / min.

7. The preparation method according to claim 3, characterized in that: include: Before the reaction, a carrier gas with a flow rate of 100 to 300 sccm is introduced into the reaction chamber for 5 to 10 minutes to remove the air in the reaction chamber; preferably, the carrier gas includes an inert gas, preferably argon; And / or, the preparation method further comprises: adjusting the flow rate of the carrier gas to 100-300 sccm, stabilizing for 1-5 minutes, and then heating to 500-800°C.

8. The preparation method according to claim 2, characterized in that: Also includes: After the reaction is completed, the temperature in the reaction chamber is rapidly reduced to room temperature, thereby obtaining two-dimensional stepped nickel oxide nanosheets; preferably, the temperature in the reaction chamber is reduced to room temperature at a rate of 30 to 50° C. / min.

9. A two-dimensional stepped nickel oxide nanosheet, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 8.

10. The two-dimensional stepped nickel oxide nanosheet according to claim 9, characterized in that: The two-dimensional stepped nickel oxide nanosheet has a stepped structure; and / or the size of the two-dimensional stepped nickel oxide nanosheet is 1 to 50 μm.

Citation Information

Cited By

  • Mica-metal oxide-based composite nano material and preparation method and application thereof

    CN119900043A

  • Mica-metal oxide composite nanomaterial, and preparation method and application thereof