Glass ceramic with high lithium content, chemically strengthened glass ceramic and application of chemically strengthened glass ceramic
By optimizing the glass formula and composition, the problem of surface cracking and peeling of high-lithium content glass in high-temperature chemical strengthening is solved, and chemically strengthened microcrystalline glass with high stress and mechanical strength is achieved, which is suitable for cover glass for electronic equipment.
Patent Information
- Application Number
- CN202410156329.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-02-02
AI Technical Summary
In the prior art, crystal crystal glass with high lithium content and containing the main crystal phase of lithium disilicate is prone to surface cracking and peeling during chemical strengthening treatment in a high-temperature salt bath, resulting in a decrease in drop resistance and mechanical strength, which cannot meet the use. Require.
By optimizing the glass formula to ensure the precipitation of lithium disilicate crystal phase and the limitations of other crystal phases, a high-lithium content microcrystalline glass is prepared, whose composition meets the specific oxide content relationship, avoids surface cracking and peeling, and improves chemistry Strengthen efficiency and maintain high stress and mechanical strength under high temperature conditions.
Chemically strengthened microcrystalline glass with high stress levels and high mechanical strength after high temperature chemical strengthening is achieved, overcoming the problems of surface cracking and peeling, improving the preparation efficiency and performance, and is suitable for cover glass for electronic equipment.
Smart Images

Figure CN118930054A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of microcrystalline glass technology, and specifically relates to a microcrystalline glass with a high lithium content, a chemically strengthened microcrystalline glass and applications thereof. Background Art
[0002] As a solid material containing microcrystalline phase and glass phase, glass-ceramics has obvious advantages in overall strength performance over conventional glass because of the large number of nano-sized crystals it contains that can hinder the expansion of micro-cracks. Currently, glass-ceramics has gradually begun to be used in portable electronic devices as cover glass of electronic devices, such as display protection glass or back cover glass.
[0003] The lithium disilicate (Li2Si2O5) crystal phase is an orthorhombic crystal based on the [Si2O5] tetrahedral array, and the shape of the crystal is flat or plate-like. Inside the glass-ceramic, the lithium disilicate crystals are randomly oriented interlocking microstructures, forcing the crack path to be distorted when passing through the crystal, thereby preventing the crack from expanding and improving the strength and fracture toughness of the glass-ceramic. At the same time, the refractive index of lithium disilicate crystals is close to that of the glass matrix (e.g., the base glass for preparing glass-ceramics), making it an ideal crystal phase for preparing highly transparent glass-ceramics. It can be seen that glass-ceramics with a main lithium disilicate crystal phase have great application potential in the cover glass market for electronic products or electronic devices. Summary of the invention
[0004] As the cover glass of electronic devices, especially the cover glass of portable electronic devices (such as mobile phones, watches, PADs, etc.), the thickness is generally less than 2mm. For example, the thickness of the cover glass of electronic devices can be about 0.1mm-2.0mm. Therefore, in order to meet the high performance requirements such as anti-fall, pressure resistance, scratch resistance, and wear resistance, it is usually necessary to chemically strengthen the cover glass of electronic devices to further improve its mechanical strength performance. The so-called "chemical strengthening" here refers to placing the glass in a molten salt bath, using the alkali metal ions with large ionic radius in the molten salt to exchange ions with the alkali metal ions with small ionic radius in the glass, thereby generating compressive stress on the glass surface. In order to improve the efficiency of chemical strengthening treatment and reduce production costs, the art generally considers using a high-temperature molten salt bath to chemically strengthen the glass.
[0005] However, for the microcrystalline glass in the prior art that has a high lithium content and contains a main crystal phase of lithium disilicate, it is easy to experience "surface cracking" and / or "peeling" when it is chemically strengthened in a high-temperature molten salt bath exceeding 480°C. The "surface cracking" here mainly refers to the large number of irregular cracks that appear on the surface of the microcrystalline glass after chemical strengthening, and the "peeling" mainly refers to the outermost layer of the microcrystalline glass falling off from the microcrystalline glass after chemical strengthening, and the thickness of the detached glass layer is between a few microns and tens of microns. The "surface cracking" phenomenon and / or "peeling" phenomenon will cause a significant reduction in the drop resistance and mechanical strength of the microcrystalline glass, and even cause the surface of the microcrystalline glass to fail after chemical strengthening and cannot be used.
[0006] The purpose of the present application is to overcome the defects of "surface cracking" and / or "peeling" in the prior art when the microcrystalline glass with high lithium content and containing lithium disilicate as the main crystal phase is chemically strengthened in a high-temperature salt bath (e.g., the salt bath temperature is above 480°C), and to provide a high-lithium-content microcrystalline glass suitable for high-temperature chemical strengthening and with lithium disilicate as the main crystal phase, a chemically strengthened microcrystalline glass and its application. After high-temperature chemical strengthening, the high-lithium-content microcrystalline glass not only overcomes the problems of "surface cracking" and / or "peeling", but also can obtain chemically strengthened microcrystalline glass with high stress level after high-temperature chemical strengthening. By adopting the high-lithium-content microcrystalline glass to carry out high-temperature chemical strengthening treatment to obtain chemically strengthened microcrystalline glass with high stress level and high mechanical strength performance, the efficiency of preparing high-strength chemically strengthened microcrystalline glass can be greatly improved.
[0007] In order to achieve the above objectives, this application provides the following technical solutions:
[0008] 1. A high lithium content glass-ceramic, wherein the high lithium content glass-ceramic comprises a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the high lithium content glass-ceramic;
[0009] Measured in terms of molar percentage of oxides, the composition of the high lithium content glass-ceramics includes:
[0010] SiO2: 41.00mol%-69.50mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol% , Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;
[0011] The composition of the high-lithium-content microcrystalline glass satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content microcrystalline glass: 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41, preferably 0.21≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.39. By optimizing the glass formula so that the components satisfy a specific content relationship and interact with each other, on the one hand, it is beneficial to ensure the precipitation of the desired content of lithium disilicate crystal phase and limit the precipitation of other crystal phases (such as petalite crystal phase), thereby helping to ensure that microcrystalline glass with high intrinsic strength and excellent optical properties and with lithium disilicate as the main crystal phase is obtained. On the other hand, it is beneficial to ensure that the microcrystalline glass satisfies a specific composition and structure, thereby ensuring that it can achieve high-temperature chemical strengthening and ensuring that it will not have "surface cracking" and / or surface "peeling" problems during the high-temperature chemical strengthening process, thereby helping to improve its chemical strengthening efficiency and can ensure that the chemically strengthened microcrystalline glass prepared thereby meets high stress levels (such as high CS_50, |CT_AV|, DOL_0, etc.) and high mechanical strength properties.
[0012] 2. The high-lithium-content glass-ceramics according to technical solution 1, wherein the composition of the high-lithium-content glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics, also satisfies: 0.25≤(2.2×ZrO2+0.35×CaO+Na2O) / Li2O≤0.45; preferably 0.27≤(2.2×ZrO2+0.35×CaO+Na2O) / Li2O≤0.43. By making the composition of the glass-ceramics satisfy this relationship, it is beneficial to ensure that the high-lithium-content glass-ceramics has high intrinsic strength and excellent optical properties, while avoiding the phenomenon of "surface cracking" and / or "peeling" when the glass-ceramics is strengthened in a high-temperature molten salt bath.
[0013] 3. The high-lithium-content glass-ceramics according to technical solution 1 or 2, wherein the composition of the high-lithium-content glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics, satisfies:
[0014] 0≤(CaO+MgO+ZnO+Na2O+K2O) / (ZrO2+Li2O)≤0.15; and / or,
[0015] 0.90≤SiO2+Li2O≤0.95; and / or,
[0016] 2.00≤SiO2 / Li2O≤2.30; and / or,
[0017] 0≤(CaO+SrO) / ZrO2≤1.50; and / or,
[0018] 0≤Al2O3 / (SiO2+Al2O3)≤0.03. By making the composition satisfy at least one of the above relationship equations, it is beneficial to further improve the structure of the glass, thereby being beneficial to preparing a high-lithium-content glass-ceramic that meets a specific structure and has excellent properties (especially optical properties, strength properties, etc.), and is also beneficial to ensuring the chemical strengthening effect of the high-lithium-content glass-ceramic, ensuring that the high-lithium-content glass-ceramic can be prepared into a chemically strengthened glass-ceramic with a high stress level, excellent mechanical strength properties, and excellent damage resistance through chemical strengthening.
[0019] It should be pointed out that in the above formulas of the present application, the content percentage is substituted into each formula in molar terms, that is, the molar unit does not participate in the calculation of the formula. For example, if the molar content of Al2O3 is 2%, 2% is substituted into the formula for calculation.
[0020] 4. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 3, wherein, in terms of molar percentage of oxides, the high-lithium-content glass-ceramics:
[0021] The content of SiO2 is 60.00mol%-65.00mol%, preferably the content of SiO2 is 61.00mol%-63.50mol%; and / or, the content of Li2O is 27.50mol%-31.00mol%, preferably the content of Li2O is 28.00mol%-30.50mol%; and / or, the content of ZrO2 is 3.00mol%-6.00mol%, preferably the content of ZrO2 is 3.50mol%-6.00mol%; and / or, the content of P2O5 is 1.50mol%-2.50mol%, preferably the content of P2O5 is 1.60mol%-2.10mol%; and / or, the content of CaO is 0.00mol%-4.00mol%, preferably the content of CaO is 0.00mol%-2.00mol%. By adjusting the composition of high-lithium-content glass-ceramics, the high-lithium-content glass-ceramics can obtain higher mechanical strength and damage resistance.
[0022] 5. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 4, wherein, in terms of the molar percentage of oxides, the composition of the high-lithium-content glass-ceramics further comprises: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, and Ta2O5: 0.00mol%-1.00mol%. In the glass system of the present application, the selective addition of an appropriate amount of Y2O3, La2O3 or Ta2O5 helps to increase the density of the high-lithium-content glass-ceramics and increase its Young's modulus, but may also increase the refractive index of the high-lithium-content glass-ceramics, thereby reducing the optical properties of the high-lithium-content glass-ceramics.
[0023] 6. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 5, wherein the composition of the high-lithium-content glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics, satisfies:
[0024] 0≤(CaO+MgO+ZnO+Na2O+K2O) / (ZrO2+Li2O)≤0.10; and / or,
[0025] 0.90≤SiO2+Li2O≤0.93; and / or,
[0026] 0≤(CaO+SrO) / ZrO2≤1.00, preferably 0≤(CaO+SrO) / ZrO2≤0.70. By making the composition satisfy at least one of the above relationship, it is beneficial to further improve the structure of the glass, and it is more beneficial to prepare chemically strengthened microcrystalline glass with a higher stress level, which is beneficial to ensure that the prepared chemically strengthened microcrystalline glass has excellent mechanical strength and damage resistance.
[0027] 7. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 6, wherein the density of the high-lithium-content glass-ceramics is ρ≥2.54 g / cm 3 , refractive index ≤1.60. High lithium content glass-ceramics that meet this density and refractive index can ensure high intrinsic strength and excellent optical properties.
[0028] 8. The high-lithium-content glass-ceramic according to any one of technical solutions 1 to 7, wherein at a thickness of 0.5 mm, the b value of the high-lithium-content glass-ceramic is ≤1.0, preferably ≤0.8. The high-lithium-content glass-ceramic that meets the optical b value can ensure better optical performance and display effects, and is suitable for use in display screens that require display effects.
[0029] 9. The high-lithium-content glass-ceramic according to any one of technical solutions 1-8, wherein the high-lithium-content glass-ceramic is transparent in the visible light range, and / or, at a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the high-lithium-content glass-ceramic is ≥ 85.00%, preferably ≥ 90.00%. The high-lithium-content glass-ceramic that meets the higher transmittance can ensure good light transmittance and good transparency, and is suitable for use in display screens that require display effects.
[0030] 10. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 9, wherein the high-lithium-content glass-ceramics has a crystallinity of 30.00wt%-90.00wt%, preferably 50.00wt%-90.00wt%. A higher content of microcrystalline phase is beneficial to improving the mechanical strength of the high-lithium-content glass-ceramics.
[0031] 11. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 10, wherein the average crystal size of the high-lithium-content glass-ceramics is ≤100nm, preferably ≤50nm, and more preferably 15nm-45nm. A smaller average crystal size is conducive to ensuring that the high-lithium-content glass-ceramics has excellent optical properties.
[0032] 12. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 11, wherein the Young's modulus of the high-lithium-content glass-ceramics is ≥100.00 GPa, preferably the Young's modulus of the high-lithium-content glass-ceramics is ≥110.00 GPa, and more preferably the Young's modulus of the high-lithium-content glass-ceramics is 114 GPa-130 GPa. A higher Young's modulus indicates that the high-lithium-content glass-ceramics has a higher intrinsic strength, which is conducive to obtaining higher mechanical strength and damage resistance.
[0033] 13. The high-lithium-content glass-ceramics according to any one of technical solutions 1 to 12, wherein the expansion softening point of the high-lithium-content glass-ceramics is 750° C.-820° C. The appropriate expansion softening point is conducive to 3D hot bending of the high-lithium-content glass-ceramics to obtain 3D curved glass-ceramics with high strength performance.
[0034] 14. A chemically strengthened glass-ceramic, wherein the composition at the center of the chemically strengthened glass-ceramic is the same as the composition of the high-lithium-content glass-ceramic described in any one of Technical Solutions 1-13, and the chemically strengthened glass-ceramic includes a compressive stress layer region extending from the surface of the chemically strengthened glass-ceramic to the compression depth, and has tensile stress inside the chemically strengthened glass-ceramic.
[0035] 15. The chemically strengthened glass-ceramics according to technical solution 14, wherein the chemically strengthened glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; and the composition at the center of the chemically strengthened glass-ceramics, measured in molar percentage of oxides, includes:
[0036] SiO2: 41.00mol%-69.50mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol% , Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;
[0037] The composition at the center of the chemically strengthened glass-ceramics satisfies the following conditions, expressed as the molar percentage of each oxide in the composition at the center of the chemically strengthened glass-ceramics: 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41, preferably 0.21≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.39.
[0038] 16. The chemically strengthened glass-ceramic according to technical solution 14 or 15, wherein the chemically strengthened glass-ceramic has a DOL_0 of 0.20t-0.25t, preferably a DOL_0 of 0.22t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramic. The DOL_0 of the chemically strengthened glass-ceramic is within the above range, indicating that the chemically strengthened glass-ceramic has a high depth of the compressive stress layer, which is beneficial for it to offset the energy driving the crack extension, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0039] 17. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 16, wherein the chemically strengthened glass-ceramic has a |CT_AV| of 80MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress; preferably, a |CT_AV| of 90MPa-200MPa; and more preferably, a |CT_AV| of 130MPa-200MPa. The |CT_AV| of the chemically strengthened glass-ceramic is within the above range, indicating that the chemically strengthened glass-ceramic has a higher tensile stress level, reflecting that it has a higher surface compressive stress level, and the higher surface compressive stress level can offset more residual energy from falling, squeezing, impact or collision, thereby ensuring that it has excellent damage resistance.
[0040] 18. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 17, wherein the chemically strengthened glass-ceramic has a CT_LD of 50000MPa / mm-100000MPa / mm, where CT_LD is a tensile stress linear density; preferably, a CT_LD of 55000MPa / mm-100000MPa / mm; and more preferably, a CT_LD of 65000MPa / mm-100000MPa / mm. The range of CT_LD of the chemically strengthened glass-ceramic is within the above range, indicating that the tensile stress stored inside the chemically strengthened glass-ceramic is relatively dense, indicating that the chemically strengthened glass-ceramic has a higher surface compressive stress level, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0041] 19. A chemically strengthened glass-ceramic according to any one of technical solutions 14 to 18, wherein the chemically strengthened glass-ceramic has a CS_50 of 150MPa-280MPa, CS_50 refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened glass-ceramic; preferably, it has a CS_50 of 160MPa-280MPa; more preferably, it has a CS_50 of 180MPa-280MPa. The range of CS_50 of the chemically strengthened glass-ceramic is within the above range, indicating that the compressive stress of the chemically strengthened glass-ceramic at a depth of 50μm from the surface is high, indicating that the chemically strengthened glass-ceramic has a higher surface compressive stress level, and the higher the surface compressive stress level, the more residual energy of falling, extrusion, impact or collision can be offset, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0042] 20. The chemically strengthened glass-ceramics according to any one of technical solutions 14 to 19, wherein the chemically strengthened glass-ceramics with a thickness of 0.5 mm is subjected to a sandpaper drop resistance test using 80-grit sandpaper, and the average sandpaper drop resistance height of the chemically strengthened glass-ceramics is ≥1.0 m, preferably ≥1.2 m, and more preferably ≥1.5 m. This indicates that the chemically strengthened glass-ceramics has excellent drop resistance.
[0043] 21. A glass device, wherein the glass device comprises the high-lithium-content microcrystalline glass as described in any one of Technical Solutions 1 to 13 or comprises the chemically strengthened microcrystalline glass as described in any one of Technical Solutions 14 to 20.
[0044] 22. An electronic device, wherein the electronic device comprises the high-lithium-content microcrystalline glass as described in any one of Technical Solutions 1-13 or comprises the chemically strengthened microcrystalline glass as described in any one of Technical Solutions 14-20.
[0045] Beneficial effects:
[0046] The present application ensures that the high-lithium-content microcrystalline glass containing the main crystalline phase lithium disilicate satisfies a specific composition and structure, especially satisfies the oxide content under specific conditions and the specific oxide content relationship, which not only ensures that it can achieve high-temperature chemical strengthening, and ensures that it will not have "surface cracking" and / or surface "peeling" problems during the high-temperature chemical strengthening process, thereby improving its chemical strengthening efficiency, but also ensures that the chemically strengthened microcrystalline glass prepared by it meets high stress levels (such as having high CS_50, |CT_AV|, DOL_0, etc.) and high mechanical strength performance. The high-lithium-content microcrystalline glass of the present application can be used to produce chemically strengthened microcrystalline glass that takes into account both excellent optical properties and mechanical strength properties, which is conducive to broadening its application scenarios and application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0048] Figure 1 This is a real picture of the chemically strengthened glass-ceramics of Example 1 under strong light.
[0049] Figure 2 This is a real picture of the chemically strengthened microcrystalline glass of Example 2 under strong light.
[0050] Figure 3 This is a morphology image of a cross section of the chemically strengthened glass-ceramic in Example 1 along the thickness direction under an optical microscope (magnification 200 times); wherein A points to the surface of the chemically strengthened glass-ceramic in Example 1, and B points to the inside of the chemically strengthened glass-ceramic in Example 1.
[0051] Figure 4 This is a real picture of the chemically strengthened micro-ceramic glass of comparative example 1 under strong light irradiation, and the chemically strengthened micro-ceramic glass has a "surface cracking" phenomenon;
[0052] Figure 4A This is a morphology image of a cross section of the chemically strengthened glass-ceramics of Comparative Example 1 along the thickness direction under an optical microscope (magnified 200 times);
[0053] Figure 4B This is a morphology image of a local area of the main surface of the chemically strengthened glass-ceramics of Comparative Example 1 under an optical microscope (magnification 50 times);
[0054] Figure 4A , Figure 4B , 1 points to the interior of the chemically strengthened glass-ceramics of Comparative Example 1, 2 points to the “crack” area on the main surface of the chemically strengthened glass-ceramics of Comparative Example 1, and 3 points to the air.
[0055] Figure 5 This is a real picture of the chemically strengthened microcrystalline glass of comparative example 12 under natural light. The chemically strengthened microcrystalline glass has a surface "peeling" phenomenon.
[0056] Figure 6 This is a morphology image of the cross-section of the chemically strengthened microcrystalline glass of Comparative Example 12 along the thickness direction under an optical microscope (magnification 50 times); wherein 4 points to the interior of the chemically strengthened microcrystalline glass of Comparative Example 12, and 5 points to the surface "peeling" area of the chemically strengthened microcrystalline glass of Comparative Example 12.
[0057] Figure 7 This is the transmittance curve of the high lithium content glass-ceramics of Example 6 in the 360nm-740nm band.
[0058] Figure 8 This is the XRD spectrum of the high lithium content microcrystalline glass of Example 6.
[0059] Fig. 9 It is the XRD spectrum of the microcrystalline glass in comparative example 1 before and after chemical strengthening; wherein, curve A is the XRD spectrum of the microcrystalline glass in comparative example 1, and curve B is the XRD spectrum of the chemically strengthened microcrystalline glass in comparative example 1.
[0060] Fig.10 It is the XRD spectrum of the high-lithium-content microcrystalline glass in Example 4 before and after chemical strengthening; wherein, curve C is the XRD spectrum of the high-lithium-content microcrystalline glass in Example 4, and curve D is the XRD spectrum of the chemically strengthened microcrystalline glass in Example 4.
[0061] Fig.11 This is a test curve of the thermal expansion coefficient of high-lithium-content glass-ceramics of Example 8. The temperature shown in the figure is the expansion softening point temperature of the high-lithium-content glass-ceramics. DETAILED DESCRIPTION
[0062] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they can be included or not (or can be included or not).
[0063] Glossary and test methods:
[0064] "Surface cracking" phenomenon: refers to the phenomenon that chemically strengthened glass (such as chemically strengthened microcrystalline glass) shows obvious cracks on the surface when exposed to strong light.
[0065] Surface "peeling" phenomenon: refers to the phenomenon that the surface glass of chemically strengthened glass (such as chemically strengthened microcrystalline glass) separates from the glass body.
[0066] Base glass: glass that has not been subjected to nucleation, crystallization or strengthening treatment.
[0067] Glass-ceramics: also known as glass ceramics, is a type of solid composite material that contains both a glass phase and a crystal phase (also called a microcrystalline phase or a crystalline phase) and is prepared by targeted and controlled crystallization of the base glass.
[0068] Chemically strengthened glass-ceramics: refers to the solid composite material obtained after chemical strengthening treatment of glass-ceramics. During high-temperature chemical strengthening treatment, the alkali metal ions with large ionic radius (such as potassium ions or sodium ions) in the molten salt bath will replace the alkali metal ions with small ionic radius (such as sodium ions or lithium ions) in the glass-ceramics, thereby generating an exchange ion volume difference and generating compressive stress (also called compression stress) on the surface of the glass-ceramics.
[0069] Nucleation: Through heat treatment, the nucleating material in the glass grows small crystal nuclei.
[0070] Crystallization: Glass grows a certain crystal based on the crystal nucleus through heat treatment.
[0071] Crystalline phase: Crystalline phase is the microscopic structure of crystals. It is a general term for a large number of crystalline solid phase components, or also called crystal.
[0072] Main crystalline phase: also known as primary crystalline phase, refers to a crystalline phase having a higher weight content than other crystalline phases present in the microcrystalline glass.
[0073] Main surface: refers to the surface with the largest surface area in the glass brick or glass sheet, such as the upper and lower surfaces of the cover glass.
[0074] Crystallinity: refers to the percentage of the total mass of the crystalline phase or crystals in the microcrystalline glass to the mass of the microcrystalline glass, or also called the total content of the crystalline phase in the microcrystalline glass.
[0075] Refractive index: The refractive index refers to the ratio of the speed of light in a vacuum to the speed of light in the medium.
[0076] Transmittance: When light of a certain wavelength is irradiated onto the glass surface, the light will be reflected, absorbed and transmitted. The ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.
[0077] SOC: Photoelastic coefficient. Photoelasticity mainly refers to the phenomenon of anisotropy and birefringence of transparent materials after being subjected to force. By measuring the photoelastic coefficient and birefringence, the value of the residual stress (in MPa) inside the material can be obtained.
[0078] CT_LD: refers to the tensile stress linear density, measured in MPa / mm. It should be understood that after the glass-ceramics is placed in a molten salt bath for ion exchange, a compressive stress layer (or also called a compressive stress layer) will be formed on the surface of the glass-ceramics, and a tensile stress layer (or also called a tensile stress layer) will be formed inside the glass-ceramics. Exemplarily, during chemical strengthening, alkali metal ions with a large radius in the molten salt bath are ion exchanged with alkali metal ions with a small radius in the glass-ceramics, thereby forming a compressive stress layer on the surface of the glass-ceramics and a tensile stress layer inside the glass-ceramics. In this application, CT_LD is calculated by the following formula:
[0079]
[0080] Wherein, t is the thickness of chemically strengthened glass-ceramics, in mm; DOL_0 is the depth of the compressive stress layer of chemically strengthened glass-ceramics, in μm; |CT_AV| is the absolute value of the average tensile stress of chemically strengthened glass-ceramics, in MPa. It should be understood that in the calculation formula of tensile stress linear density, the data is substituted into the calculation according to the above unit requirements, and the calculation result is obtained, and the unit does not participate in the calculation.
[0081] CS_50: refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened microcrystalline glass, in MPa.
[0082] |CT_AV|: refers to the absolute value of the average tensile stress, in MPa, specifically the absolute value of the average value of all tensile stresses in the tensile stress layer, obtained by testing with the SLP-2000 stress meter.
[0083] DOL_0: refers to the depth of the compressive stress layer, or the depth of the compressive stress layer, specifically the distance from any main surface of the chemically strengthened microcrystalline glass to the position close to the surface where the compressive stress is zero, obtained by testing with the SLP-2000 stress meter.
[0084] b value: used to characterize the yellow-blue value of a material. The optical b value in the present invention is the b value of transmitted light, and a positive optical b value indicates that the material is blue.
[0085] Upper limit temperature of crystallization: The upper limit temperature of crystallization refers to the highest temperature at which the substrate glass produces crystallization. Above this temperature, the substrate glass will not precipitate crystals.
[0086] Thickness of glass: measured by micrometer. It should be understood that in the thickness direction, the degree of ion exchange changes gradually from the surface to the center, and the total Na-K and / or Li-Na exchange amount generally does not exceed 1.5% of the total mass of the sample, and the difference in ion radius is at the pm level, so the expansion effect in the thickness direction is extremely slight, and it can be approximately considered that the thickness has basically not changed. That is, the thickness change of microcrystalline glass before and after chemical strengthening is very small and can be ignored.
[0087] Glass sheet size specification measurement: tested using a two-dimensional measuring machine (instrument model: Miyu MY-YXCL-4030).
[0088] XRD test: The high lithium content microcrystalline glass or chemically strengthened microcrystalline glass of the present application is crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample is tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the incident angle range used in the test is 2θ=10°-50°, the scanning speed is 6° / min, the operating voltage is 40 kV, and the operating current is 30 mA.
[0089] Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.
[0090] Determination of crystallinity: The XRD test results (RAW format) are imported into the X-ray diffraction data Rietveld refinement software Jade for fitting and calculation to determine the crystallinity of the sample. Specifically, the ratio of the fitted crystalline phase peak area to the fitted total peak area is recorded as the crystallinity of the sample.
[0091] Determination of average crystal size: Using the result data obtained from the XRD test, the average crystal size of the sample can be calculated according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the X-ray wavelength, λ = 0.154056nm, β is the half-height width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW format file output by the XRD instrument is curve fitted in the Jade software, and Jade outputs a fitting report. According to the angle 2θ value and PeakFWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted into radians: β = (FWHM / 180×3.14), and the crystal size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size in the sample.
[0092] Test of transmittance and optical b-value: With reference to the national standard "GB / T 7962.12-2010 Test method for colorless optical glass Part 12: Spectral transmittance", a haze meter is used to test the transmittance and optical b-value of the high lithium content microcrystalline glass of this application. Specifically, a haze meter is used to test the transmittance and optical b-value of 5 microcrystalline glasses of the same batch to light of different wavelengths. The average value of the optical b-values measured for the 5 microcrystalline glasses is taken and recorded as the optical b-value result of the microcrystalline glass. The average value of the transmittance measured for the 5 microcrystalline glasses under 550nm wavelength light is taken and recorded as the transmittance result of the microcrystalline glass under 550nm wavelength light. Among them, the haze meter used in the test of this application is the Konica Minolta spectrophotometer CM-3600A from Japan, the light receiving optical system is transmission, the spectroscopic method is a plane reflective grating, the wavelength range is 360nm-740nm, the wavelength spacing is 10nm, the illumination light source is a pulsed xenon lamp X4, the ambient temperature of the instrument is 24°C, and the air humidity is 40%.
[0093] Density: This application uses the electronic density balance SD-200L of Japan ALFAMIRAGE to test the density of high lithium content microcrystalline glass.
[0094] Refractive index: This application uses a WYA-2WAJ Abbe refractometer to measure the refractive index of high lithium content glass-ceramics.
[0095] Exchange amount: refers to the ratio of the mass difference of high-lithium-content glass-ceramics before and after chemical strengthening to the mass of high-lithium-content glass-ceramics before chemical strengthening.
[0096] Expansion softening point temperature: The sample is made into a cylinder with a diameter of 5.5mm and a length of 20mm. The sample is tested using a thermal expansion instrument LINSEIS L75VD1000. The test outputs a thermal expansion coefficient test curve. The corresponding temperature when the curve begins to decrease with increasing temperature is the expansion softening point temperature of the sample.
[0097] Young's modulus: The UMS-100 ultrasonic material characterization system was used to test the Young's modulus of high lithium content glass-ceramics by sound waves.
[0098] Crystallization upper limit temperature: Break the substrate glass into small pieces, then put them into the long quartz tank and cover them. Set the temperature range of the gradient furnace model JKZC-XJY01, such as the temperature range of 1050℃-1225℃, and take at least 6 temperature points from high to low in each temperature range. After the gradient furnace reaches the preset temperature range, put the long quartz tank with the sample into the gradient furnace, so that the 6 temperature points correspond to the glass samples at 6 positions in the long quartz tank, and place the long quartz tank in the gradient furnace for 60-70 minutes at a constant temperature, and then take out the long quartz tank. Use a microscope and a magnifying glass to observe the glass samples at different positions in the long quartz tank. If the glass sample is devitrified or foggy, it is determined that the glass sample at that location is crystallized. If the glass sample is completely transparent, it is determined that the glass sample at that location is not crystallized. The crystallization upper limit temperature range is between the temperature point corresponding to the completely transparent sample and the temperature point corresponding to the adjacent devitrified or foggy sample. The average value of the two temperature points is taken as the crystallization upper limit temperature. If all or none of the glass samples in the long quartz tank crystallize within the temperature range set by the gradient furnace, the temperature range of the gradient furnace is reset to measure the upper limit temperature of crystallization of the glass samples.
[0099] Average sandpaper drop height test: The average sandpaper drop height of the chemically strengthened glass-ceramics of the same embodiment or the same comparative example is calculated by adding up the measured sandpaper drop height of each sample and dividing it by the number of samples measured. This value is recorded as the average sandpaper drop height of the tested chemically strengthened glass-ceramics, which is used to characterize the drop damage resistance of the chemically strengthened glass-ceramics. At least 10 samples are taken from each batch for testing, and the average sandpaper drop height is calculated.
[0100] Where n is the number of glass samples tested in each batch, hi is the sandpaper drop resistance height of a single sample test;
[0101] Among them, the test method for the sandpaper drop height of a single sample is:
[0102] Step 1: Stick 80-grit sandpaper on the lower surface of the 181g model machine, and place the model machine on the green figure LT-SKDL-CD drop machine;
[0103] Step 2: Place a chemically strengthened glass-ceramic sample to be tested with a length, width and thickness of 50mm×50mm×0.5mm directly below the model machine, with the chemically strengthened glass-ceramic sample facing the sandpaper. Make the model machine fall from a certain drop height to impact the chemically strengthened glass-ceramic sample directly below the model machine. If the chemically strengthened glass-ceramic sample does not break, increase the drop height of the model machine in a certain pattern, and make the model machine continue to fall, impacting the chemically strengthened glass-ceramic sample directly below the model machine, until the chemically strengthened glass-ceramic sample breaks. For example, the drop height of the model machine starts from 0.4m, and the sample is dropped once. If the sample does not break, the drop height of the model machine is increased by 0.1m, and it falls again. Repeat the above process until the chemically strengthened glass-ceramic sample breaks;
[0104] Step 3: The last drop height of the chemically strengthened microcrystalline glass sample before it breaks is recorded as its anti-sandpaper drop height. For example, if the drop height is increased by 0.1m each time, when the drop height of the sample is 0.5m when it breaks, the anti-sandpaper drop height of the sample is 0.4m.
[0105] Without being bound by any theory, it is speculated that the chemical strengthening process of microcrystalline glass usually goes through the following two steps: first, ion exchange occurs at the interface between microcrystalline glass and molten salt, and ions with larger ionic radius in the molten salt enter the microcrystalline glass; second, the large-radius ions exchanged in the microcrystalline glass migrate deeper into the microcrystalline glass. However, in the prior art, when microcrystalline glass with a high lithium content and containing a main crystalline phase of lithium disilicate is chemically strengthened in a high-temperature salt bath (e.g., a salt bath temperature above 480°C), surface ion exchange (e.g., lithium ions Li in the microcrystalline glass) occurs. + With the sodium ion Na in the salt bath + The rate of exchange) is relatively fast, while the migration rate of large-radius ions entering through exchange is limited by the internal structure of the microcrystalline glass. In this case, the compressive stress generated on the surface of the microcrystalline glass will quickly reach its bearing limit, which can easily lead to "surface cracking" on the surface of the microcrystalline glass. The "surface cracking" phenomenon mainly occurs on the first main surface and / or the second main surface of the microcrystalline glass, and the cracks do not penetrate the entire depth or thickness of the microcrystalline glass.
[0106] Furthermore, when the chemical strengthening treatment is carried out at a higher temperature, the first main surface or / and the second main surface of the microcrystalline glass with a high lithium content and containing a main crystalline phase of lithium disilicate may even be prone to "peeling", that is, the outermost layer will directly fall off from the microcrystalline glass, and the thickness of the detached layer will usually be from a few microns to tens of microns.
[0107] The "surface cracking" and / or "peeling" of the microcrystalline glass that occurs during the chemical strengthening process is very harmful to the performance of the microcrystalline glass itself. It will not only cause the surface of the microcrystalline glass to fail, but also greatly reduce the mechanical strength of the microcrystalline glass, making it unable to meet the requirements of use.
[0108] In view of this, the present application provides a high-lithium-content glass-ceramic suitable for high-temperature chemical strengthening and having lithium disilicate as the main crystalline phase, a chemically strengthened glass-ceramic and its application. After high-temperature chemical strengthening, the high-lithium-content glass-ceramic not only overcomes the problem of "surface cracking" and / or surface "peeling", but also can obtain chemically strengthened glass-ceramic with high stress performance after high-temperature chemical strengthening. By adopting the high-lithium-content glass-ceramic for high-temperature chemical strengthening treatment to prepare chemically strengthened glass-ceramic with high stress level and high mechanical strength performance, the efficiency of preparing high-strength chemically strengthened glass-ceramic can be greatly improved.
[0109] As described above, in some embodiments of the present application, a high-lithium-content glass-ceramic is provided, wherein the high-lithium-content glass-ceramic contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the high-lithium-content glass-ceramic; in terms of molar percentage of oxides, the composition of the high-lithium-content glass-ceramic includes: SiO2: 41.00mol%-69.50mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, Zn O: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%; measured by the content expressed in molar percentage of each oxide in the composition of the high lithium content microcrystalline glass, the composition of the high lithium content microcrystalline glass satisfies: 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41.
[0110] In the present application, by optimizing the glass formula, such as using a higher content of zirconium and a lower content of aluminum at a higher content of lithium, and so on, while ensuring that the various components satisfy a specific content relationship and interact with each other, on the one hand, it is beneficial to ensure the precipitation of the desired content of lithium disilicate crystalline phase and limit the precipitation of other crystalline phases (such as petalite crystalline phase), thereby helping to ensure that a microcrystalline glass with high intrinsic strength and excellent optical properties and with lithium disilicate as the main crystalline phase is obtained; on the other hand, it is beneficial to ensure that the microcrystalline glass meets a specific composition and structure, thereby ensuring that it can achieve high-temperature chemical strengthening, ensuring that it will not have "surface cracking" and / or surface "peeling" problems during the high-temperature chemical strengthening process, thereby helping to improve its chemical strengthening efficiency, and can ensure that the chemically strengthened microcrystalline glass prepared by it has a high stress level (such as high CS_50, |CT_AV|, DOL_0, etc.) and high mechanical strength properties.
[0111] In some embodiments, the value of 2.25×Li2O-8×ZrO2-0.2×CaO can be, for example, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40 or 0.41, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.
[0112] In the glass system of the present application, SiO2 is a glass network forming oxide and an indispensable component of the glass network structure. Properly increasing the content of SiO2 can increase the structural stability and mechanical strength of the glass, but excessive SiO2 will increase the viscosity of the substrate glass, making the glass melting more difficult, thereby reducing the formability of the substrate glass. Therefore, the molar percentage of SiO2 is controlled at 41.00mol%-69.50mol%, preferably, the molar percentage of SiO2 is 60.00mol%-65.00mol%, and more preferably 61.00mol%-64.00mol%.
[0113] In some embodiments, the high lithium content glass-ceramics may contain 41.00mol%-69.50mol%, 42.00mol%-69.00mol%, 50.00mol%-68.00mol%, 55.00mol%-66.00mol%, 60.00mol%-69.00mol%, 60.00mol%-65.00mol%, 61.00mol%-69.00mol%, 61.00mol%-64.00mol%, 62.00mol%-64.00mol%, 63.00mol%-64.00mol%, 61.00mol%-63.50mol% or 63.00mol%-69.50mol% SiO2. In some embodiments, the high lithium content glass-ceramics may contain 41.00 mol%, 42.00 mol%, 43.00 mol%, 44.00 mol%, 45.00 mol%, 46.00 mol%, 47.00 mol%, 50.00 mol%, 53.00 mol%, 55.00 mol%, 58.00 mol%, 60.00 mol%, 61.00 mol%, 62.00 mol%, 63.00 mol%, 63.50 mol%, 64.00 mol%, 65.00 mol% or 69.50 mol% SiO2, or SiO2 within the numerical range formed by any two of the above specific numerical values as endpoints, as long as high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content microcrystalline glass or chemically strengthened microcrystalline glass having the required performance of the present application can be obtained.
[0114] In the glass system of the present application, Al2O3 is an optional component. The addition of an appropriate amount of Al2O3 helps to promote the exchange of ions during the chemical strengthening process to a certain extent, but excessive Al2O3 will increase the viscosity of the glass and easily lead to the precipitation of other crystalline phases, such as petalite, etc., which affects the crystalline structure of the microcrystalline glass. Therefore, the molar percentage of Al2O3 is controlled at 0.00mol%-2.00mol%.
[0115] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-2.00mol%, 0.00mol%-1.60mol%, 0.00mol%-1.00mol%, 0.50mol%-1.60mol%, 0.50mol%-1.00mol%, 0.00mol%-0.50mol%, 1.20mol%-1.60mol%, 0.00mol%-1.30mol%, 0.00mol%-1.20mol% or 1.00mol%-2.00mol% Al2O3. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol% of Al2O3, or Al2O3 within the numerical range formed by any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0116] In the glass system of the present application, P2O5, as a nucleating agent, is an indispensable part. When its content is too little or too much, it will lead to poor crystallization effect and affect the optical properties of the obtained microcrystalline glass, such as reducing the transparency of the microcrystalline glass. Therefore, the molar percentage of P2O5 is controlled at 1.50mol%-3.00mol%, preferably 1.50mol%-2.10mol%.
[0117] In some embodiments, the high lithium content glass-ceramics may contain 1.50mol%-3.00mol%, 1.60mol%-2.80mol%, 1.50mol%-2.50mol%, 1.60mol%-2.10mol%, 1.70mol%-2.20mol%, 1.50mol%-1.60mol%, 1.70mol%-3.00mol%, 1.60mol%-2.50mol%, 1.70mol%-2.30mol%, 1.80mol%-2.00mol%, 2.00mol%-3.00mol%, 1.80mol%-1.90mol%, 1.60mol%-1.90mol%, 1.70mol%-1.90mol%, 1.75mol%-1.95mol% or 1.50mol%-2.10mol% of P2O5. In some embodiments, the high lithium content glass-ceramics may contain 1.50mol%, 1.60mol%, 1.70mol%, 1.75mol%, 1.80mol%, 1.85mol%, 1.95mol%, 2.00mol%, 2.10mol%, 2.20mol%, 2.30mol%, 2.40mol%, 2.50mol%, 2.60mol%, 2.80mol% or 3.00mol% of P2O5, or P2O5 within a numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0118] In the glass system of the present application, ZrO2 is an intermediate oxide in the formation of glass. An appropriate amount of ZrO2 can improve the chemical stability of the glass, increase the hardness of the glass, and increase the scratch and drop resistance of the glass. At the same time, due to the high cationic charge and strong field strength of ZrO2, it has a large accumulation effect on the glass structure and is often used as a nucleating agent in microcrystalline glass. In the present application, the use of a certain amount of ZrO2 is not only beneficial for the microcrystalline glass to obtain higher stress after chemical strengthening, but also beneficial for the microcrystalline glass to resist "surface cracking" during the strengthening process. However, too high a ZrO2 content will cause glass phase separation or be detrimental to obtaining microcrystalline glass with excellent optical properties. Therefore, the molar percentage of ZrO2 is controlled at 2.00mol%-6.00mol%, preferably 3.00mol%-6.00mol%.
[0119] In some embodiments, the high lithium content glass-ceramics may contain 2.00mol%-6.00mol%, 2.30mol%-5.80mol%, 2.50mol%-5.50mol%, 2.80mol%-5.30mol%, 2.90mol%-5.10mol%, 3.00mol%-5.50mol%, 3.10mol%-4.80mol%, 4.80mol%-6.00mol%, 4.00mol%-5.80mol%, 3.20mol%-5.30mol%, 3.50mol%-5.00mol%, 3.50mol%-6.00mol%, 3.50mol%-5.80mol%, 4.00mol%-5.00mol% or 3.00mol%-6.00mol%. In some embodiments, the high lithium content glass-ceramics may contain 2.00mol%, 2.30mol%, 2.50mol%, 2.70mol%, 2.90mol%, 3.00mol%, 3.10mol%, 3.30mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 5.80mol% or 6.00mol% ZrO2, or ZrO2 within the numerical range formed by any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0120] In the glass system of the present application, CaO is an optional component of the network exosome oxide formed by the glass. An appropriate amount of CaO helps to reduce the high temperature viscosity of the glass and increase the density of the glass, but an excessive amount of CaO will shorten the material properties of the glass and increase its brittleness. In the present application, the appropriate addition of a small amount of CaO helps to increase the stress obtained by the microcrystalline glass after chemical strengthening, and also slows down the chemical strengthening rate of the microcrystalline glass. Therefore, the molar percentage of CaO is controlled at 0.00mol%-5.00mol%, preferably 0.00mol%-4.00mol%.
[0121] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-5.00mol%, 0.10mol%-4.00mol%, 0.00mol%-4.00mol%, 0.50mol%-3.80mol%, 0.80mol%-2.00mol%, 0.00mol%-1.60mol%, 0.00mol%-1.00mol%, 1.50mol%-4.00mol%, 0.00mol%-2.00mol%, 1.00mol%-4.00mol% or 0.10mol%-5.00mol% CaO. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.10 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol%, 2.00 mol%, 3.00 mol%, 4.00 mol% or 5.00 mol% CaO, or CaO in a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0122] In the glass system of the present application, Li2O is an essential component and a network exo-oxide formed by glass. It can not only improve the viscosity of the glass and promote the melting and clarification of the glass liquid, but also is one of the main components for forming lithium disilicate crystals. At the same time, Li2O can also provide alkali metal lithium ions for ion exchange with large-radius ions in the molten salt bath, which is an important factor affecting the stress level that can be obtained by chemically strengthened microcrystalline glass. However, excessive Li2O will deteriorate the optical properties of microcrystalline glass and easily cause the microcrystalline glass to produce "surface cracking" during the strengthening process. Therefore, the molar percentage of Li2O is controlled at 27.00mol%-32.00mol%, preferably 27.00mol%-30.00mol%.
[0123] In some embodiments, the high lithium content glass-ceramics may contain 27.00 mol%-32.00 mol%, 27.50 mol%-31.00 mol%, 27.00 mol%-30.00 mol%, 27.50 mol%-29.50 mol%, 28.00 mol%-32.00 mol%, 28.50 mol%-31.00 mol%, 29.00 mol%-30.50 mol%, 28.00 mol%-30.50 mol% or 29.50 mol%-32.00 mol% Li2O. In some embodiments, the high lithium content glass-ceramics may contain 27.00mol%, 27.50mol%, 28.00mol%, 28.50mol%, 29.00mol%, 29.50mol%, 30.00mol%, 30.50mol%, 31.00mol%, 31.50mol% or 32.00mol% of Li2O, or Li2O within a numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0124] In the glass system of the present application, MgO is an optional component. An appropriate amount of MgO can adjust the glass phase composition in the microcrystalline glass. However, excessive MgO will affect the growth of crystals and the crystalline structure of the microcrystalline glass. Therefore, the molar percentage of MgO is controlled at 0.00 mol%-2.00 mol%.
[0125] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-2.00mol%, 0.00mol%-1.60mol%, 0.50mol%-1.60mol%, 0.80mol%-1.50mol%, 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.10mol%-1.10mol%, 0.10mol%-1.50mol% or 0.00mol%-1.40mol% MgO. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol% of MgO, or MgO within a numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0126] In the glass system of the present application, ZnO is one of the optional components as a network intermediate. An appropriate amount of ZnO can combine with free oxygen to adjust the glass structure, and can remain in the glass phase of the microcrystalline glass to increase the glass viscosity. However, excessive ZnO will affect the growth of crystals and the crystal phase structure of the microcrystalline glass. Therefore, the molar percentage of ZnO is controlled to be between 0.00mol% and 2.00mol%.
[0127] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-2.00mol%, 0.00mol%-1.70mol%, 0.50mol%-1.60mol%, 0.80mol%-1.50mol%, 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.10mol%-1.10mol%, 0.10mol%-1.50mol% or 0.00mol%-1.40mol% ZnO. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol% of ZnO, or ZnO within the numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0128] In the glass system of the present application, Na2O is an optional component and a network exo-oxide. An appropriate amount of Na2O can provide free oxygen, improve the viscosity of the glass, promote the melting and clarification of the glass liquid, and also adjust the chemical strengthening rate. However, excessive Na2O will not only reduce the crystallinity of the microcrystalline glass, but also affect the chemical strengthening effect. Therefore, the molar percentage of Na2O is controlled to be between 0.00mol% and 3.00mol%.
[0129] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-3.00mol%, 0.00mol%-2.80mol%, 0.00mol%-1.00mol%, 0.10mol%-2.70mol%, 0.50mol%-1.60mol%, 0.60mol%-1.00mol%, 2.50mol%-3.00mol% or 0.00mol%-0.50mol% Na2O. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol%, 2.00 mol%, 2.50 mol% or 3.00 mol% of Na2O, or Na2O within a numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0130] In the glass system of the present application, K2O is an oxide outside the glass network and is one of the optional components. An appropriate amount of K2O can provide free oxygen to increase the oxygen-silicon ratio in the glass structure, but too much K2O will affect the network structure of the glass, and affect the optical properties, thermal stability, chemical stability, mechanical strength and weather resistance of the glass. Therefore, the molar percentage of K2O is controlled to be between 0.00 mol% and 1.00 mol%.
[0131] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-1.00mol%, 0.50mol%-1.00mol%, 0.00mol%-0.50mol%, 0.85mol%-1.00mol% or 0.00mol%-0.15mol% K2O. In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%, 0.15mol%, 0.50mol%, 0.70mol%, 0.85mol%, 0.95mol% or 1.00mol% K2O, or K2O within the numerical range formed by any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0132] In the glass system of the present application, B2O3 is an optional component. An appropriate amount of B2O3 can be used as a flux and / or softener to help improve the molding and hot bending effects of the glass. However, excessive B2O3 will cause uncontrollable crystallization process and deteriorate the optical properties of the microcrystalline glass. Therefore, the molar percentage of B2O3 is controlled at 0.00mol%-1.00mol%.
[0133] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.50mol%-1.00mol%, 0.10mol%-0.85mol%, 0.85mol%-1.00mol% or 0.25mol%-0.75mol% B2O3. In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%, 0.10mol%, 0.25mol%, 0.50mol%, 0.60mol%, 0.70mol%, 0.75mol%, 0.85mol%, 0.95mol% or 1.00mol% B2O3, or B2O3 within the numerical range formed by any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content microcrystalline glass or chemically strengthened microcrystalline glass having the required performance of the present application can be obtained.
[0134] In the glass system of the present application, SrO is an alkaline earth metal oxide as an optional component. An appropriate amount of SrO can play a role in regulating the glass phase composition in the microcrystalline glass, which helps to increase the density of the microcrystalline glass and increase its Young's modulus. At the same time, it is also beneficial to reduce the expansion softening point of the microcrystalline glass, and then facilitate the hot bending of the microcrystalline glass into 3D curved microcrystalline glass. However, excessive SrO will deteriorate the optical properties of the microcrystalline glass, so the molar percentage of SrO is controlled at 0.00mol%-2.00mol%.
[0135] In some embodiments, the high lithium content glass-ceramics may contain 0.00mol%-2.00mol%, 0.10mol%-2.00mol%, 0.00mol%-1.00mol%, 0.10mol%-1.00mol%, 0.30mol%-1.90mol%, 0.40mol%-1.20mol%, 1.20mol%-2.00mol%, 0.00mol%-0.30mol%, 0.85mol%-1.40mol%, 0.85mol%-1.90mol%, 0.50mol%-1.20mol% or 1.00mol%-2.00mol% SrO. In some embodiments, the high lithium content glass-ceramics may contain 0.00 mol%, 0.30 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol% of SrO, or SrO within a numerical range consisting of any two of the above specific numerical values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0136] In some embodiments, the composition of the high lithium content glass-ceramics includes, in terms of molar percentage of oxides: SiO2: 60.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-4.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%. By making the microcrystalline glass meet the above-mentioned composition, it is not only beneficial to give the high-lithium-content microcrystalline glass with lithium disilicate as the main crystalline phase high intrinsic strength and excellent optical properties, but also beneficial to ensure its chemical strengthening effect, ensuring that the microcrystalline glass obtains a higher stress level after chemical strengthening, and thus obtains higher mechanical strength and damage resistance.
[0137] In some embodiments, the composition of the high lithium content glass-ceramics described in the present application may further include other components on the basis of the above composition range. For example, in some specific embodiments, the composition of the high lithium content glass-ceramics further includes, in terms of molar percentage of oxides: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.
[0138] In the glass system of the present application, the selective addition of an appropriate amount of Y2O3, La2O3 or Ta2O5 helps to increase the density of the microcrystalline glass and increase its Young's modulus, but it may also increase the refractive index of the microcrystalline glass and reduce the optical properties of the microcrystalline glass. Therefore, the molar percentage of Y2O3, La2O3 or Ta2O5 is controlled at 0.00mol%-1.00mol%.
[0139] In some embodiments, in the high lithium content glass-ceramics, the molar percentage of Y2O3, La2O3 or Ta2O5 can be 0.00mol%, 0.10mol%, 0.20mol%, 0.30mol%, 0.40mol%, 0.50mol%, 0.60mol%, 0.70mol%, 0.80mol%, 0.85mol%, 0.90mol%, 0.95mol% or 1.00mol%, or a value within the numerical range formed by any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0140] In some embodiments, the composition of the high lithium content glass-ceramics includes, in terms of molar percentage of oxides: SiO2: 60.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-2.50mol%, ZrO2: 3.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3. 00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.50mol%-31.00mol%, CaO: 0.00mol%-2.50mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%, Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%. By making the high lithium content microcrystalline glass meet the above composition, it is more conducive to preparing chemically strengthened microcrystalline glass with a higher stress level, and further conducive to ensuring that the prepared chemically strengthened microcrystalline glass has high mechanical strength and excellent damage resistance.
[0141] In some embodiments of the present application, the composition of the high-lithium-content glass-ceramics also satisfies the following conditions: 0.25≤(2.2×ZrO2+0.35×CaO+Na2O) / Li2O≤0.45, based on the content expressed as the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics. By making the composition of the glass-ceramics satisfy this relationship, it is beneficial to ensure that the high-lithium-content glass-ceramics have high intrinsic strength and excellent optical properties while avoiding the phenomenon of "surface cracking" and / or "peeling" of the glass-ceramics during chemical strengthening in a high-temperature molten salt bath. In some embodiments, the value of (2.2×ZrO2+0.35×CaO+Na2O) / Li2O can be, for example, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44 or 0.45, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.
[0142] In some embodiments of the present application, the composition of the high-lithium-content glass-ceramics also satisfies the following conditions: 0.00≤(CaO+MgO+ZnO+Na2O+K2O) / (ZrO2+Li2O)≤0.15, based on the content expressed by the molar percentage of each oxide in the high-lithium-content glass-ceramics composition. The use of a composition and structure that satisfies this relationship will be more conducive to improving the stress level generated by the high-lithium-content glass-ceramics after chemical strengthening. In some embodiments, the value of (CaO + MgO + ZnO + Na2O + K2O) / (ZrO2 + Li2O) can be, for example, 0.00, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14 or 0.15, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained.
[0143] In some embodiments of the present application, the composition of the high-lithium-content glass-ceramics also satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics: 0.90≤SiO2+Li2O≤0.95. The use of a composition and structure that satisfies this relationship is conducive to ensuring that the desired content of lithium disilicate crystals is precipitated in the glass-ceramics, and can effectively reduce the precipitation of other crystals, such as petalite crystals, which is conducive to ensuring that the glass-ceramics obtains higher intrinsic strength and optical properties, and is also conducive to enabling the glass-ceramics to obtain a high stress level after chemical strengthening. At the same time, it is also conducive to ensuring that the substrate glass does not lose transparency when the glass-ceramics is prepared by heat treatment, or that the substrate glass does not lose transparency during the melting process. In some embodiments, the value of SiO2+Li2O may be, for example, 0.900, 0.904, 0.905, 0.910, 0.915, 0.920, 0.925, 0.930, 0.935, 0.940, 0.945 or 0.950, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained.
[0144] In some embodiments of the present application, the composition of the high-lithium-content glass-ceramics also satisfies the following conditions: 2.00≤SiO2 / Li2O≤2.30, measured by the content expressed as the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics. The use of a composition and structure that satisfies this relationship is conducive to reducing the crystal size of the glass-ceramics and improving the optical properties of the glass-ceramics; at the same time, it is conducive to ensuring the precipitation of the main crystalline phase lithium disilicate crystals and can effectively reduce the precipitation of other crystalline phases, such as petalite crystals, which is conducive to ensuring that the glass-ceramics obtains a higher intrinsic strength and is also conducive to obtaining a high stress level for the glass-ceramics after chemical strengthening. In some embodiments, the value of SiO2 / Li2O may be, for example, 2.00, 2.02, 2.04, 2.06, 2.08, 2.10, 2.12, 2.14, 2.16, 2.18, 2.20, 2.22, 2.24, 2.26, 2.28, or 2.30, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as a high lithium content glass-ceramic or chemically strengthened glass-ceramic with the performance required by the present application can be obtained.
[0145] In some embodiments of the present application, the composition of the high lithium content glass-ceramics is also satisfied by the content expressed as the molar percentage of each oxide in the composition of the high lithium content glass-ceramics: 0≤(CaO+SrO) / ZrO2≤1.50. The use of a composition and structure that satisfies this relationship will be more conducive to improving the stress level generated by the high lithium content glass-ceramics after chemical strengthening. In some embodiments, the value of (CaO+SrO) / ZrO2 can be, for example, 0.00, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.00, 1.20, 1.30, 1.40 or 1.50, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content microcrystalline glass or chemically strengthened microcrystalline glass having the required performance of the present application can be obtained.
[0146] In some embodiments of the present application, the composition of the high-lithium-content glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the high-lithium-content glass-ceramics, also satisfies: 0≤Al2O3 / (SiO2+Al2O3)≤0.03. The use of a composition and structure that satisfies this relationship is more conducive to ensuring the precipitation of the main crystalline phase lithium disilicate crystals, and can effectively reduce the precipitation of other crystalline phases, such as petalite crystals, which is conducive to ensuring that the glass-ceramics obtains higher intrinsic strength and optical properties, and is also conducive to making the glass-ceramics obtain a high stress level after chemical strengthening. In some embodiments, the value of Al2O3 / (SiO2+Al2O3) can be, for example, 0.00, 0.01, 0.020, 0.022, 0.023, 0.024, 0.025 or 0.03, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the high-lithium-content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content microcrystalline glass or chemically strengthened microcrystalline glass having the required performance of the present application can be obtained.
[0147] In some embodiments, the composition of the high lithium content glass-ceramics satisfies the following conditions, based on the content expressed as a molar percentage of each oxide in the high lithium content glass-ceramics composition:
[0148] 0≤(CaO+MgO+ZnO+Na2O+K2O) / (ZrO2+Li2O)≤0.10; and / or,
[0149] 0.90≤SiO2+Li2O≤0.93; and / or,
[0150] 0≤(CaO+SrO) / ZrO2≤1.00, preferably 0≤(CaO+SrO) / ZrO2≤0.70. By making the composition satisfy at least one of the above relationship, it is beneficial to further improve the structure of the glass, and it is more beneficial to prepare chemically strengthened microcrystalline glass with a higher stress level, which is beneficial to ensure that the prepared chemically strengthened microcrystalline glass has high mechanical strength and excellent damage resistance.
[0151] The high-lithium content microcrystalline glass of the present application has a specific composition and structure, and can achieve high-temperature chemical strengthening. When it is chemically strengthened in a high-temperature molten salt bath, there will be no "surface cracking" and / or "peeling" phenomenon. In some embodiments of the present application, in a mixed salt bath at 500°C, after being treated for 1h-5h, there is no diffraction peak in the X-ray diffraction spectrum of the high-lithium content microcrystalline glass in the range of 35.30°-35.90° at 2θ; wherein the mixed salt bath includes 29.99wt% NaNO3, 69.98wt% KNO3 and 0.03wt% LiNO3.
[0152] It should be pointed out that after the above-mentioned treatment for 1h-5h, there is no diffraction peak in the range of 2θ of 35.30°-35.90° in the X-ray diffraction spectrum of the high-lithium content microcrystalline glass, which means that at any time between the treatment of 1h-5h, there is no diffraction peak in the range of 2θ of 35.30°-35.90° in the X-ray diffraction spectrum.
[0153] In some embodiments of the present application, the density of the high lithium content glass-ceramics is ρ≥2.54 g / cm 3 , refractive index ≤1.60. High lithium content glass-ceramics that meet this density and refractive index can ensure high intrinsic strength and excellent optical properties.
[0154] In some embodiments, the density ρ of the high lithium content glass-ceramics may be 2.54 g / cm 3 , 2.55g / cm 3 , 2.56g / cm 3 , 2.57g / cm 3 , 2.58g / cm 3 , 2.59g / cm 3 , 2.60g / cm 3 , 2.61g / cm 3 , 2.62g / cm 3 , 2.63g / cm 3 , 2.64g / cm 3 or 2.65g / cm 3, or a value greater than any of the above specific values, or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0155] In some embodiments, the refractive index of the high lithium content glass-ceramics can be 1.50, 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59 or 1.60, or a value below any of the above specific values, or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0156] In some embodiments of the present application, at a thickness of 0.5 mm, the b value of the high lithium content glass-ceramics is ≤1.0, preferably ≤0.8. The high lithium content glass-ceramics that meets the optical b value can ensure better optical performance and display effects, and is suitable for use in display screens that require display effects. In some embodiments, at a thickness of 0.5 mm, the b value of the high lithium content glass-ceramics can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0, or a value below any of the above specific values, or a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0157] In some embodiments of the present application, the high-lithium-content glass-ceramics is transparent in the visible light range, and / or, at a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the high-lithium-content glass-ceramics is ≥ 85.00%, preferably ≥ 90.00%. Glass-ceramics with a high lithium content that meets this transmittance can ensure good light transmittance and transparency, and is suitable for use in display screens that require display effects. The "visible light range" here refers to light in the 360nm-740nm band.
[0158] In some embodiments, at a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the high lithium content glass-ceramics can be 85.00%, 86.00%, 87.00%, 88.00%, 89.00%, 90.00%, 90.50%, 91.00% or 92.00%, or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0159] The high-lithium-content microcrystalline glass of the present application has a high transmittance and a low b value, both of which indicate that the high-lithium-content microcrystalline glass of the present application has excellent optical properties and good uniformity, is in a transparent state, and can meet the application requirements of cover glass for electronic devices.
[0160] In some embodiments of the present application, the crystallinity of the high lithium content glass-ceramics is 30.00wt%-90.00wt%, preferably 50.00wt%-90.00wt%. The "crystallization of glass-ceramics" here refers to the percentage of the content of all crystalline phases or crystals in the glass-ceramics to the mass of the glass-ceramics. A higher content of microcrystalline phase is beneficial to improving the mechanical strength properties of glass-ceramics. In some embodiments, the crystallinity of the high lithium content glass-ceramics can be 30.00wt%-90.00wt%, 45.00wt%-85.00wt%, 50.00wt%-90.00wt%, 55.00wt%-85.00wt%, 60.00wt%-85.00wt%, 65.00wt%-90.00wt%, 70.00wt%-90.00wt% or 68.00wt%-85.00wt%. In some embodiments, the crystallinity of the high lithium content glass-ceramics can be 30.00wt%, 35.00wt%, 40.00wt%, 45.00wt%, 50.00wt%, 55.00wt%, 60.00wt%, 65.00wt%, 70.00wt%, 75.00wt%, 80.00wt%, 85.00wt% or 90.00wt%, or a value within the numerical range formed by any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0161] In some embodiments of the present application, "the main crystalline phase is lithium disilicate" or "the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the high lithium content microcrystalline glass" and similar expressions mean that the lithium disilicate crystalline phase accounts for more than 70 weight percent (wt %) of all crystalline phases of the microcrystalline glass according to the embodiments of the present application.
[0162] In some embodiments of the present application, non-limiting examples of other possible crystalline phases in the high-lithium content glass-ceramics include: petalite crystalline phase, and / or, lithium phosphate crystalline phase. In some embodiments, the high-lithium content glass-ceramics further comprises a petalite crystalline phase, preferably the weight percentage of the petalite crystalline phase in the glass-ceramics is ≤20%, more preferably, the weight percentage of the petalite crystalline phase in the glass-ceramics can be ≤15%, ≤10%, or ≤5%.
[0163] In some embodiments of the present application, in the high lithium content glass-ceramics, the average crystal size is ≤100nm, preferably the average crystal size is ≤50nm, and more preferably the average crystal size is 15nm-45nm. Meeting the smaller average crystal size is conducive to ensuring the excellent optical properties of glass-ceramics. In some embodiments, the average crystal size can be 10nm-100nm, 20nm-90nm, 30nm-80nm, 40nm-60nm, 10nm-30nm, 10nm-20nm, 5nm-35nm or 15nm-35nm. In some embodiments, the average crystal size can be 10nm, 15nm, 20nm, 30nm, 40nm, 45nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, or a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a high lithium content microcrystalline glass or chemically strengthened microcrystalline glass having the required performance of the present application can be obtained.
[0164] In some embodiments of the present application, the upper crystallization temperature of the substrate glass corresponding to the high-lithium content glass-ceramics is between 1000° C. and 1100° C. Meeting this upper crystallization temperature range is conducive to the industrial mass production of high-lithium content glass-ceramics.
[0165] In some embodiments of the present application, the Young's modulus of the high lithium content glass-ceramics is ≥100.00GPa, preferably the Young's modulus of the high lithium content glass-ceramics is ≥110.00GPa, and more preferably the Young's modulus of the high lithium content glass-ceramics is 114GPa-130GPa. Having a higher Young's modulus indicates that the high lithium content glass-ceramics has a higher intrinsic strength, which is beneficial for it to obtain higher mechanical strength properties. In some embodiments, the Young's modulus of the high lithium content glass-ceramics can be 100.00GPa-150.00GPa, 105.00GPa-140.00GPa, 110.00GPa-130.00GPa or 114.00GPa-125.00GPa. In some embodiments, the Young's modulus of the high lithium content glass-ceramics can be 100.00GPa, 105.00GPa, 110.00GPa, 114GPa, 115.00GPa, 120.00GPa, 125.00GPa, 130.00GPa, 140.00GPa or 150.00GPa, or a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.
[0166] In some embodiments of the present application, the expansion softening point of the high lithium content glass-ceramics is between 750°C and 820°C. A suitable expansion softening point is conducive to the 3D hot bending of the high lithium content glass-ceramics to obtain 3D curved glass-ceramics with high strength performance. In some embodiments, the expansion softening point of the high lithium content glass-ceramics can be 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C or 820°C, or a value within the numerical range formed by any two of the above specific values as endpoints, as long as the high lithium content glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the high lithium content glass-ceramics with the performance required by the present application can be obtained.
[0167] In the present application, the high lithium content glass-ceramics can be prepared into 3D curved glass-ceramics after heat bending. The composition of the 3D curved glass-ceramics is the same or substantially the same as that of the high lithium content glass-ceramics in terms of molar percentage of oxides.
[0168] The high-lithium-content glass-ceramics of the present application can be prepared by heat treating a substrate glass, and the composition of the substrate glass used is the same or substantially the same as that of the high-lithium-content glass-ceramics in terms of the molar percentage of oxide.
[0169] In the present application, the substrate glass can be prepared by the molding method in the prior art, and the present application has no restrictions on this. For example, the molding method may include but is not limited to: float, overflow, rolling or pouring, etc. Exemplarily, the raw materials and the clarifier can be mixed evenly (the uniformity is above 98%), melt-molded and annealed to obtain the substrate glass. Further, the process parameters may include: the melting temperature is 1480℃-1680℃, the annealing temperature is 450℃-650℃, and the annealing temperature is kept at 10h-48h. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of the clarifier added may be 0-1wt% of the total amount of the raw materials.
[0170] In the present application, when the substrate glass is heat-treated to prepare a high-lithium content microcrystalline glass, the heat treatment can be carried out in an annealing furnace, for example, and the heat treatment method can include but is not limited to one-step heat treatment, two-step heat treatment or multi-step heat treatment, for example, it can include a two-step heat treatment of nucleation treatment and then crystallization treatment. The process conditions of the heat treatment may include but are not limited to: the nucleation temperature can be 500℃-600℃, the nucleation holding time can be 120min-360min; the crystallization temperature can be 600℃-800℃, and the crystallization holding time can be 60min-180min; the heating rate of the whole process can be 5℃ / min-20℃ / min, and the cooling rate can be 0.1℃ / min-3℃ / min. After the heat treatment, those skilled in the art can also perform other conventional steps to obtain a high-lithium content microcrystalline glass sample that meets the required specifications or requirements, such as cutting, CNC processing (computer numerical control, i.e., CNC machine tools) or polishing.
[0171] In the present application, a chemically strengthened glass-ceramic is also provided, wherein the composition at the center of the chemically strengthened glass-ceramic is the same as the composition of the high-lithium-content glass-ceramic described above, the chemically strengthened glass-ceramic includes a compressive stress layer region extending from the surface of the chemically strengthened glass-ceramic to the compression depth, and has tensile stress inside the chemically strengthened glass-ceramic.
[0172] It should be understood that the composition of the surface of the glass-ceramic article after chemical strengthening may be different from the composition of the glass-ceramic before it undergoes the ion exchange process. This is because, during the ion exchange process, one type of alkali metal ion (e.g., Li + Or Na + ) are replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced. However, in an embodiment, the glass composition and phase assembly at the depth center or near the depth center of the microcrystalline glass product will still have the composition and phase assembly of the newly formed microcrystalline glass. That is to say, in the present application, the composition (e.g., the composition of the tensile stress layer) and phase assembly at the center of the chemically strengthened microcrystalline glass that has been chemically strengthened are the same or substantially the same as those of the newly formed high-lithium content microcrystalline glass.
[0173] In the present application, the chemically strengthened glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; in terms of molar percentage of oxides, the composition at the center of the chemically strengthened glass-ceramics includes: SiO2: 41.00mol%-69.50mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3. 00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%; based on the content of each oxide expressed in molar percentage in the composition at the center of the chemically strengthened microcrystalline glass, the composition at the center of the chemically strengthened microcrystalline glass satisfies: 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41, preferably 0.21≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.39.
[0174] In some embodiments of the present application, the chemically strengthened glass-ceramics has a DOL_0 of 0.20t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramics. In some embodiments, the depth of the compressive stress layer DOL_0 of the chemically strengthened glass-ceramics may be 0.20t-0.25t, 0.21t-0.24t, 0.21t-0.25t or 0.22t-0.25t. Exemplarily, when the thickness of the chemically strengthened glass-ceramics is 0.5 mm, the DOL_0 of the chemically strengthened glass-ceramics may be 0.100 mm, 0.105 mm, 0.110 mm, 0.112 mm, 0.113 mm, 0.114 mm, 0.115 mm, 0.116 mm, 0.117 mm, 0.118 mm, 0.119 mm, 0.120 mm, 0.121 mm, 0.122 mm, 0.123 mm, 0.124 mm or 0.125 mm, or a value within the numerical range formed by any two of the above specific values as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The DOL_0 of the chemically strengthened glass-ceramics is within the above range, indicating that the chemically strengthened glass-ceramics has a high depth of compressive stress layer, which is more conducive to offsetting the energy driving crack propagation, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0175] In some embodiments of the present application, the chemically strengthened glass-ceramics has a |CT_AV| of 80MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress; preferably, it has a |CT_AV| of 90MPa-200MPa. In some embodiments, the chemically strengthened glass-ceramics has a |CT_AV| of 80MPa-200MPa, 90MPa-200MPa, 90MPa-180MPa, 100MPa-150MPa, 130MPa-180MPa, 80MPa-100MPa, 85MPa-120MPa, 90MPa-150MPa, 95MPa-180MPa, 100MPa-140MPa, or 120MPa-140MPa. In some embodiments, the chemically strengthened glass-ceramics has a |CT_AV| of 80MPa, 90MPa, 100MPa, 110MPa, 120MPa, 130MPa, 140MPa, 150MPa, 160MPa, 170MPa, 180MPa, 190MPa or 200MPa, or a |CT_AV| within a numerical range consisting of any two of the above specific values as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The |CT_AV| of the chemically strengthened glass-ceramics is within the above range, indicating that the chemically strengthened glass-ceramics has a higher tensile stress level, reflecting that it has a higher surface stress level, and the higher surface compressive stress level can offset the more residual energy of falling, extrusion, impact or collision, thereby ensuring that it has excellent damage resistance.
[0176] In some embodiments of the present application, the chemically strengthened glass-ceramics has a CT_LD of 50000 MPa / mm-100000 MPa / mm, where CT_LD is a tensile stress linear density; preferably, it has a CT_LD of 55000 MPa / mm-100000 MPa / mm. In some embodiments, the chemically strengthened glass-ceramics has a CT_LD of 50000MPa / mm-100000MPa / mm, 55000MPa / mm-95000MPa / mm, 60000MPa / mm-90000MPa / mm, 65000MPa / mm-85000MPa / mm, 70000MPa / mm-80000MPa / mm, 65000MPa / mm-100000MPa / mm, 60000MPa / mm-80000MPa / mm or 60000MPa / mm-100000MPa / mm. In some embodiments, the chemically strengthened glass-ceramics has a CT_LD of 50000MPa / mm, 55000MPa / mm, 60000MPa / mm, 65000MPa / mm, 70000MPa / mm, 75000MPa / mm, 80000MPa / mm, 85000MPa / mm, 90000MPa / mm, 95000MPa / mm or 100000MPa / mm, or a CT_LD within a numerical range consisting of any two of the above specific values as endpoints, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. The range of CT_LD of the chemically strengthened glass-ceramics is within the above range, indicating that the tensile stress stored inside the chemically strengthened glass-ceramics is relatively dense, indicating that the chemically strengthened glass-ceramics has a higher surface stress level, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0177] In some embodiments of the present application, the chemically strengthened glass-ceramics has a CS_50 of 150MPa-280MPa, where CS_50 refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened glass-ceramics; preferably, it has a CS_50 of 160MPa-280MPa. In some embodiments, the chemically strengthened glass-ceramics has a CS_50 of 150MPa-280MPa, 160MPa-270MPa, 165MPa-265MPa, 170MPa-260MPa, 180MPa-280MPa, 165MPa-250MPa, or 180MPa-200MPa. In some embodiments, the chemically strengthened glass-ceramics has a CS_50 of 150MPa, 160MPa, 170MPa, 180MPa, 190MPa, 200MPa, 210MPa, 220MPa, 230MPa, 240MPa, 250MPa, 260MPa, 270MPa or 280MPa, or a CS_50 within a numerical range consisting of any two of the above specific values as endpoints, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. The range of CS_50 of the chemically strengthened glass-ceramics is within the above range, indicating that the compressive stress of the chemically strengthened glass-ceramics at a depth of 50 μm from the surface is high, indicating that the chemically strengthened glass-ceramics has a higher surface stress level, and the higher the surface compressive stress level can offset more residual energy from falling, extrusion, impact or collision, thereby ensuring that it has excellent damage resistance, such as excellent drop resistance.
[0178] In the present application, by making the chemically strengthened glass-ceramics meet specific stress characteristics, it can be ensured that the chemically strengthened glass-ceramics has excellent mechanical strength properties, excellent mechanical strength properties and excellent damage resistance, especially excellent drop damage resistance.
[0179] In some embodiments of the present application, 80 mesh sandpaper is used to perform an anti-sandpaper drop test on the chemically strengthened glass-ceramics with a thickness of 0.5 mm, and the average anti-sandpaper drop height of the chemically strengthened glass-ceramics is ≥1.0m, preferably the average anti-sandpaper drop height is ≥1.2m, and more preferably the average anti-sandpaper drop height is ≥1.5m. This shows that the chemically strengthened glass-ceramics of the present application has excellent anti-drop performance. In some embodiments, 80 mesh sandpaper is used to perform an anti-sandpaper drop test on the chemically strengthened glass-ceramics with a thickness of 0.5 mm, and the average anti-sandpaper drop height of the chemically strengthened glass-ceramics can be 1.0m, 1.1m, 1.2m, 1.3m, 1.4m, 1.5m, 1.6m, 1.7m, 1.8m, 1.9m, 2.0m or 2.1m, etc.
[0180] The chemically strengthened glass-ceramics of the present application can be obtained by chemically strengthening the high-lithium-content glass-ceramics described above. The chemical strengthening process can be carried out with reference to the process in the prior art, and may include, for example, first heating the molten salt containing a certain sodium ion concentration to the temperature required for chemical strengthening, and then preheating the high-lithium-content glass-ceramics (for example, a heating rate of 5°C / min-100°C / min can be used during preheating) to the required chemical strengthening temperature and then placing it in the molten salt. After constant temperature treatment until the time required for chemical strengthening is achieved, taking it out, cooling it to room temperature, cleaning the salt attached to the surface, and drying it to obtain a chemically strengthened glass-ceramics with a high stress level.
[0181] In some embodiments of the present application, the temperature of the molten salt bath for chemical strengthening treatment can be 400°C-530°C, and the time of chemical strengthening treatment can be 0.5h-24h. In some embodiments of the present application, the composition of the molten salt includes 4.8wt%-100wt% sodium salt, 0-95wt% potassium salt and 0-0.2wt% lithium salt in terms of mass ratio. Furthermore, the selected sodium salt, potassium salt and lithium salt can be nitrate, sulfate, phosphate or carbonate, etc. In some embodiments, after the chemical strengthening treatment is completed, when the chemically strengthened microcrystalline glass is cooled, the cooling rate can be 1°C / min-50°C / min.
[0182] The high-lithium-content microcrystalline glass or chemically strengthened microcrystalline glass with excellent performance provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), vehicle-mounted central control, electronic whiteboard glass, smart home, and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device of microcrystalline glass required. For example, it can be used for display screens, cover glass, touch screens, glass inner screens or inner frames of electronic devices; for example, it can be used for windshields of vehicles, aircraft or aircraft, such as front windshields or side windshields. For example, it can be used for work surfaces, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces may include but are not limited to exterior wall surfaces, stair tread surfaces, column veneers or counter surfaces, etc. Storage containers may include but are not limited to cups, plates, medicine bottles or beverage bottles, etc.
[0183] The embodiments of the present application are described in detail below, which are exemplary and are only used to explain the present application, and should not be construed as limiting the present application.
[0184] In the example numbers of the following tables, S refers to an embodiment, such as S1 refers to Example 1; D refers to a comparative example, such as D1 refers to Comparative Example 1.
[0185] Example 1
[0186] (1) Preparation of substrate glass:
[0187] Prepare raw materials with a total mass of 1000g (the raw materials are configured according to the formula of S1 in Table 1, and the proportions of each oxide are shown in Table 2), and add 5g of sodium chloride to the configured raw materials, mix at a speed of 25r / min in a V-type mixer for 30min, and melt in a platinum crucible at 1650℃ for 5h, then pour into a mold to form a glass brick, cool to 900℃, put into a 460℃ annealing furnace for annealing for 12h, and then cool to room temperature with the furnace to obtain a base material glass brick.
[0188] (2) Preparation of high-lithium content microcrystalline glass: The substrate glass brick is placed in an annealing furnace, and the temperature is raised from room temperature to 525°C at a rate of 10°C / min for nucleation treatment. After heat preservation at this temperature for 240 minutes, the temperature is raised to 685°C at a rate of 10°C / min for crystallization treatment. The temperature is kept at this temperature for 60 minutes, and then the temperature is cooled to room temperature at a rate of 1°C / min to obtain a high-lithium content microcrystalline glass brick. The composition of the obtained high-lithium content microcrystalline glass is the same as that of the substrate glass in terms of molar percentage of oxides, as shown in Tables 1 and 2 for details.
[0189] The obtained high-lithium-content microcrystalline glass sample brick is subjected to cold working treatments of cutting, CNC processing (the CNC instrument model used in this application is: RCG500S), and polishing in sequence, and a high-lithium-content microcrystalline glass sample that meets the required specifications and requirements can be obtained. In this application, the high-lithium-content microcrystalline glass sample brick is subjected to the above-mentioned cold working treatment to be made into a high-lithium-content microcrystalline glass sample with a thickness of 0.50 mm, specifically, a microcrystalline glass polished sheet sample of 50 mm×50 mm×0.50 mm is made.
[0190] Test results of the high lithium content glass-ceramic sample obtained in S1:
[0191] The main crystal phase composition, crystallinity, average crystal size, density, refractive index, Young's modulus of the high lithium content glass-ceramics sample, as well as the optical b value and transmittance (under 550nm wavelength light) of the high lithium content glass-ceramics sample with a thickness of 0.5mm were tested respectively, and the results are shown in Table 3.
[0192] (3) Preparation of chemically strengthened glass-ceramics: The obtained high-lithium content glass-ceramics sample is placed in the strengthening furnace cavity for preheating for 5 minutes. After preheating, it is quickly placed in a 500°C molten salt for chemical strengthening. The composition of the molten salt is 29.99wt% NaNO3+69.98wt% KNO3+0.03wt% LiNO3. After chemical strengthening for 4.75 hours, the glass sample is taken out and placed on the strengthening furnace body to slowly cool to room temperature. The salt wrapped on the glass surface is washed off with clean water. After the glass sample is dried, the chemically strengthened glass-ceramics can be obtained.
[0193] Test results of chemically strengthened glass-ceramics obtained from S1:
[0194] Ⅰ. To determine whether the chemically strengthened microcrystalline glass has "surface cracks": shine a 500-2000 lumen light on the glass surface. Figure 4 If bright silk cracks are observed, it means that the chemically strengthened microcrystalline glass has "surface cracks"; or a large number of irregular cracks are observed on the surface of the chemically strengthened microcrystalline glass under an optical microscope, such as Figure 4B , it can also be said that the chemically strengthened microcrystalline glass has "surface cracks", which is recorded as the appearance of "surface cracks". If the glass surface does not have the aforementioned bright silk cracks and irregular cracks, it means that the chemically strengthened microcrystalline glass does not have "surface cracks" in appearance, which is recorded as "good". The effect of the chemically strengthened microcrystalline glass of this embodiment under strong light irradiation is as follows Figure 1 As shown in FIG. 1 , the morphology of the cross section of the chemically strengthened glass-ceramics along the thickness direction under an optical microscope (magnified 200 times) is as follows: Figure 3 As shown, it can be seen that the aforementioned bright silk seam does not exist, and there are no irregular cracks inside and on the surface of the glass. The appearance results are recorded as shown in Table 4.
[0195] Ⅱ. If the chemically strengthened glass-ceramics indicates that there is no "surface cracking", the chemically strengthened glass-ceramics is placed on a SLP2000 (Luceo, Japan) stress meter (the light source wavelength used is 518 nm, SOC = 25.5 (nm / cm) / MPa, the refractive index is set according to the refractive index value of the glass-ceramics, the refractive index of the high lithium content glass-ceramics of S1 is 1.5600, and the exposure time is 300 μsec) to measure CS_50, DOL_0, |CT_AV|; then the tensile stress line density (CT_LD) value is calculated. The results are shown in Table 4.
[0196] III. The average sandpaper drop resistance height of chemically strengthened glass-ceramics was tested. The results are shown in Table 4.
[0197] Example 2-Example 14
[0198] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each example are shown in Tables 1 to 4, respectively.
[0199] The effect of the chemically strengthened microcrystalline glass of Example 2 under strong light irradiation is as follows: Figure 2 As shown, there are no shiny silk seams and the appearance quality is good.
[0200] The XRD spectrum comparison diagram of the high lithium content glass-ceramics of Example 4 and the chemically strengthened glass-ceramics prepared from the high lithium content glass-ceramics is as follows: Fig.10 As shown, it can be seen that there is no obvious difference in the XRD spectrum of the high lithium content microcrystalline glass in Example 4 before and after chemical strengthening treatment.
[0201] In Example 6, the transmittance of the obtained high lithium content glass-ceramics in the 360nm-740nm band is as follows: Figure 7 As shown, the X-ray diffraction pattern (i.e., XRD pattern) of the high lithium content glass-ceramics is as follows Figure 8 As shown, it can be seen that the main crystalline phase of the high-lithium content glass-ceramics is the lithium disilicate crystalline phase, which is transparent in the visible light range and has high transmittance.
[0202] In Example 8, the thermal expansion coefficient test curve of the obtained high lithium content glass-ceramics is as follows: Fig.11 As shown, it can be seen that the expansion softening point temperature of the high lithium content microcrystalline glass is 777°C, indicating that the high lithium content microcrystalline glass is easier to perform 3D hot bending.
[0203] Comparative Example 1-Comparative Example 15
[0204] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each comparative example are shown in Tables 5 to 8, respectively.
[0205] Among them, in Comparative Example 1, the comparison of the XRD spectra of the microcrystalline glass before and after chemical strengthening is as follows: Fig. 9 As shown, it can be seen that after the glass-ceramics in Comparative Example 1 is chemically strengthened in a high-temperature salt bath to obtain chemically strengthened glass-ceramics, the structure undergoes obvious changes. Specifically, in the range of 2θ of 35.30°-35.90°, the glass-ceramics before chemical strengthening has no diffraction peak, but the chemically strengthened glass-ceramics prepared by it has a diffraction peak. The effect of the chemically strengthened glass-ceramics of Comparative Example 1 under strong light irradiation is shown in FIG. Figure 4 As shown, the effect under an optical microscope is as follows Figure 4A and Figure 4B As shown, it can be seen that after the microcrystalline glass in Comparative Example 1 was chemically strengthened in a high-temperature salt bath, it had the problem of "surface cracking", that is, there were a large number of "cracks" on the surface of the chemically strengthened microcrystalline glass obtained.
[0206] The chemically strengthened microcrystalline glass of Comparative Example 12 has a "peeling" phenomenon on its surface. Figure 5 Its effect under an optical microscope is shown as Figure 6 As shown, it can be seen that its surface is "peeling".
[0207] The chemically strengthened glass-ceramics of Comparative Examples 1 to 11 all showed "surface cracking" phenomenon, and the chemically strengthened glass-ceramics of Comparative Example 12 showed "peeling" phenomenon on the surface. Such chemically strengthened glass-ceramics obviously did not meet the use requirements, so the stress distribution data and exchange amount were not tested and calculated. Since the glass-ceramics of Comparative Example 13 had devitrification problem (i.e., its transmittance at 550nm was less than 85%), no subsequent testing and chemical strengthening were performed.
[0208] Crystallization upper limit temperature test: In order to analyze the industrial mass production feasibility of the high-lithium content microcrystalline glass of the present application, the crystallization upper limit temperature of the substrate glass of some embodiments was tested. Among them, the crystallization upper limit temperature of the substrate glass of S3 was 1067.2°C, and the crystallization upper limit temperature of the substrate glass of S4 was 1053.5°C, both lower than 1100°C. The crystallization upper limit temperature was between 1000°C and 1100°C, indicating that the high-lithium content microcrystalline glass of the present application is conducive to industrial mass production.
[0209] Expansion softening point test: In order to analyze the 3D hot bending effect of the high-lithium-content microcrystalline glass in the present application, the thermal expansion coefficient test curves of the high-lithium-content microcrystalline glass in some embodiments were tested, and the expansion softening point was obtained. See Table 3 for details. From the test results, it can be seen that the expansion softening point of the high-lithium-content microcrystalline glass in the present application is lower than 820°C, and is between 750°C-820°C, indicating that the high-lithium-content microcrystalline glass in the present application is conducive to 3D hot bending forming to prepare 3D curved microcrystalline glass.
[0210] Table 1
[0211]
[0212] Table 2
[0213]
[0214] Note: In Table 2, the percentage of content in terms of oxide moles is substituted into each formula, that is, the molar unit does not participate in the calculation of the formula.
[0215] Table 3
[0216]
[0217] Note: In Table 3, “ / ” means not detected.
[0218] Table 4
[0219]
[0220] Table 5
[0221]
[0222]
[0223] Table 6
[0224]
[0225] Note: In Table 6, the percentage of content in terms of oxide moles is substituted into each formula, that is, the molar unit does not participate in the calculation of the formula.
[0226] Table 7
[0227]
[0228]
[0229] Note: In Table 7, “ / ” means not tested.
[0230] Table 8
[0231]
[0232] Note: In Table 8, “ / ” means not tested.
[0233] It can be seen from the results of the embodiments of Tables 1 to 4 and the comparative examples of Tables 5 to 8 that, relative to the comparative example, the embodiment scheme of the present application, while satisfying the content range of each oxide, also satisfies the composition characteristics of: 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41. The obtained high-lithium content microcrystalline glass is suitable for high-temperature chemical strengthening, and can obtain high stress performance after high-temperature chemical strengthening. The chemically strengthened microcrystalline glass will not have "surface cracking" and / or "peeling". At the same time, the chemically strengthened microcrystalline glass has excellent optical properties, has higher CS_50, |CT_AV|, DOL_0, CT_LD, and has excellent drop resistance.
[0234] In the schemes of Comparative Examples 1 to 15, the glass formulas do not simultaneously meet the following requirements: the content range of each oxide in the present application, and the composition characteristics of 0.20≤2.25×Li2O-8×ZrO2-0.2×CaO≤0.41. After the obtained high-lithium content microcrystalline glass is chemically strengthened at high temperature, the obtained chemically strengthened microcrystalline glass either has "surface cracking" and / or "peeling" phenomenon, or has poor optical properties or stress properties. Among them, in the schemes of Comparative Examples 1 to 11, the obtained chemically strengthened microcrystalline glass has "surface cracking", the chemically strengthened microcrystalline glass of Comparative Example 12 has "peeling", the microcrystalline glass of Comparative Example 13 has devitrification and poor optical properties, and the stress properties of Comparative Examples 14 and 15 are poor.
[0235] The preferred embodiments of the present application are described in detail above, but the present application is not limited thereto. Within the technical concept of the present application, the technical solution of the present application can be subjected to a variety of simple modifications, including combining various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed in the present application and belong to the protection scope of the present application.
Claims
1. A high lithium content glass-ceramic, It is characterized in that The high-lithium-content glass-ceramics comprises a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the high-lithium-content glass-ceramics; Measured in terms of molar percentage of oxides, the composition of the high lithium content glass-ceramics includes: SiO 2 :41.00mol%-69.50mol%,Al 2 O 3 :0.00mol%-2.00mol%,P 2 O 5 :1.50mol%-3.00mol%,ZrO 2 :2.00mol%-6.00mol%,MgO:0.00mol%-2.00mol%,ZnO:0.00mol%-2.00mol%,Na 2 O:0.00mol%-3.00mol%,K 2 O:0.00mol%-1.00mol%,Li 2 O:27.00mol%-32.00mol%,CaO:0.00mol%-5.00mol%,B 2 O 3 :0.00mol%-1.00mol%,SrO:0.00mol%-2.00mol%; The composition of the high lithium content microcrystalline glass satisfies the following conditions: 0.20≤2.25×Li 2 O-8×ZrO 2 -0.2×CaO≤0.41, preferably 0.21≤2.25×Li 2 O-8×ZrO 2 -0.2×CaO≤0.
39.
2. The high lithium content glass-ceramic according to claim 1, It is characterized in that The composition of the high lithium content glass-ceramics also satisfies the following requirements: 0.25≤(2.2×ZrO 2 +0.35×CaO+Na 2 O) / Li 2 O≤0.45; preferably 0.27≤(2.2×ZrO 2 +0.35×CaO+Na 2 O) / Li 2 O≤0.
43.
3. The high lithium content glass-ceramics according to claim 1 or 2, It is characterized in that The composition of the high-lithium-content glass-ceramics satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the high-lithium-content glass-ceramics composition: 0≤(CaO+MgO+ZnO+Na 2 O+K 2 O) / (ZrO 2 +Li 2 O)≤0.15;sum / or, 0.90≤SiO 2 +Li 2 O≤0.95; and / or, 2.00≤SiO 2 / Li 2 O ≤ 2.30; and / or, 0≤(CaO+SrO) / ZrO 2 ≤1.50; and / or, 0≤Al 2 The 3 / (SiO 2 +Al 2 The 3 )≤0.03。 4. The high lithium content glass-ceramic according to any one of claims 1 to 3, It is characterized in that In terms of molar percentage of oxides, the high lithium content glass-ceramics comprises: SiO 2 The content is 60.00mol%-65.00mol%, preferably SiO 2 The content of is 61.00mol%-63.50mol%; and / or, Li 2 The content of O is 27.50mol%-31.00mol%, preferably Li 2 The content of O is 28.00mol%-30.50mol%; and / or, ZrO 2 The content of ZrO is 3.00mol%-6.00mol%, preferably ZrO 2 The content of is 3.50mol%-6.00mol%; and / or, P 2 O 5 The content of P is 1.50mol%-2.50mol%, preferably P 2 O 5 The content of is 1.60mol%-2.10mol%; and / or, The content of CaO is 0.00 mol% to 4.00 mol%, preferably the content of CaO is 0.00 mol% to 2.00 mol%.
5. The high lithium content glass-ceramic according to any one of claims 1 to 4, It is characterized in that In terms of molar percentage of oxide, the composition of the high lithium content glass-ceramics further includes: Y 2 O 3 : 0.00mol%-1.00mol%, La 2 O 3 : 0.00mol%-1.00mol%, Ta 2 O 5 : 0.00mol%-1.00mol%.
6. The high lithium content glass-ceramic according to any one of claims 1 to 5, It is characterized in that The composition of the high-lithium-content glass-ceramics satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the high-lithium-content glass-ceramics composition: 0≤(CaO+MgO+ZnO+Na 2 O+K 2 O) / (ZrO 2 +Li 2 O)≤0.10;sum / or, 0.90≤SiO 2 +Li 2 O ≤ 0.93; and / or, 0≤(CaO+SrO) / ZrO 2 ≤1.00, preference 0≤(CaO+SrO) / ZrO 2 ≤ 0.
70.
7. The high lithium content glass-ceramic according to any one of claims 1 to 6, It is characterized in that The density of the high lithium content glass-ceramics is ρ≥2.54 g / cm 3 , refractive index ≤1.
60.
8. The high lithium content glass-ceramic according to any one of claims 1 to 7, It is characterized in that At a thickness of 0.5 mm, the b value of the high lithium content glass-ceramics is ≤1.0, preferably ≤0.8; and / or, The high lithium content glass-ceramics is transparent in the visible light range, and / or, At a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the high-lithium-content microcrystalline glass is ≥85.00%, preferably ≥90.00%.
9. The high lithium content glass-ceramic according to any one of claims 1 to 8, It is characterized in that The high lithium content glass-ceramics has a crystallinity of 30.00wt%-90.00wt%, preferably a crystallinity of 50.00wt%-90.00wt%; and / or, In the high lithium content glass-ceramics, the average crystal size is ≤100 nm, preferably the average crystal size is ≤50 nm, and more preferably the average crystal size is 15 nm-45 nm.
10. The high lithium content glass-ceramic according to any one of claims 1 to 9, It is characterized in that The Young's modulus of the high-lithium-content glass-ceramics is ≥100.00 GPa, preferably the Young's modulus of the high-lithium-content glass-ceramics is ≥110.00 GPa, and more preferably the Young's modulus of the high-lithium-content glass-ceramics is 114 GPa-130 GPa.
11. A chemically strengthened glass-ceramic, It is characterized in that The composition at the center of the chemically strengthened glass-ceramics is the same as the composition of the high-lithium-content glass-ceramics described in any one of claims 1-10, and the chemically strengthened glass-ceramics includes a compressive stress layer region extending from the surface of the chemically strengthened glass-ceramics to the compression depth, and has tensile stress inside the chemically strengthened glass-ceramics.
12. The chemically strengthened glass-ceramics according to claim 11, It is characterized in that The chemically strengthened glass-ceramics includes a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; and the composition at the center of the chemically strengthened glass-ceramics, measured in molar percentage of oxides, includes: SiO 2 :41.00mol%-69.50mol%,Al 2 O 3 :0.00mol%-2.00mol%,P 2 O 5 :1.50mol%-3.00mol%,ZrO 2 :2.00mol%-6.00mol%,MgO:0.00mol%-2.00mol%,ZnO:0.00mol%-2.00mol%,Na 2 O:0.00mol%-3.00mol%,K 2 O:0.00mol%-1.00mol%,Li 2 O:27.00mol%-32.00mol%,CaO:0.00mol%-5.00mol%,B 2 O 3 :0.00mol%-1.00mol%,SrO:0.00mol%-2.00mol%; The composition at the center of the chemically strengthened glass-ceramics satisfies the following conditions: 0.20≤2.25×Li 2 O-8×ZrO 2 -0.2×CaO≤0.41, preferably 0.21≤2.25×Li 2 O-8×ZrO 2 -0.2×CaO≤0.
39.
13. The chemically strengthened glass-ceramics according to claim 11 or 12, It is characterized in that The chemically strengthened glass-ceramics has a DOL_0 of 0.20t-0.25t, preferably a DOL_0 of 0.22t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramics.
14. The chemically strengthened glass-ceramics according to any one of claims 11 to 13, It is characterized in that The chemically strengthened glass-ceramics has a |CT_AV| of 80MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress; preferably, it has a |CT_AV| of 90MPa-200MPa; and more preferably, it has a |CT_AV| of 130MPa-200MPa.
15. The chemically strengthened glass-ceramics according to any one of claims 11 to 14, It is characterized in that The chemically strengthened glass-ceramics has a CT_LD of 50000MPa / mm-100000MPa / mm, where CT_LD is the tensile stress linear density; preferably has a CT_LD of 55000MPa / mm-100000MPa / mm; more preferably has a CT_LD of 65000MPa / mm-100000MPa / mm.
16. The chemically strengthened glass-ceramics according to any one of claims 11 to 15, It is characterized in that The chemically strengthened microcrystalline glass has a CS_50 of 150MPa-280MPa, where CS_50 refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened microcrystalline glass; preferably, it has a CS_50 of 160MPa-280MPa; and more preferably, it has a CS_50 of 180MPa-280MPa.
17. The chemically strengthened glass-ceramics according to any one of claims 11 to 16, It is characterized in that Using 80-mesh sandpaper, the chemically strengthened microcrystalline glass with a thickness of 0.5 mm was subjected to a sandpaper drop resistance test. The average sandpaper drop resistance height of the chemically strengthened microcrystalline glass was ≥1.0 m, preferably the average sandpaper drop resistance height was ≥1.2 m, and more preferably the average sandpaper drop resistance height was ≥1.5 m.
18. A glass device, It is characterized in that The glass device comprises the high-lithium-content glass-ceramics according to any one of claims 1 to 10 or comprises the chemically strengthened glass-ceramics according to any one of claims 11 to 17.
19. An electronic device, It is characterized in that The electronic device comprises the high lithium content glass-ceramics according to any one of claims 1 to 10 or comprises the chemically strengthened glass-ceramics according to any one of claims 11 to 17.
Citation Information
Patent Citations
Zirconia-toughened glass ceramics
CN109476532A
Precursor glasses and transparent glass-ceramic articles formed therefrom and having improved mechanical durability
US20220402809A1
Crystallized glass, method for producing same, chemically strengthened glass, and electronic device
WO2023032937A1
Cited By
High-lithium-content glass-ceramic, chemically strengthened glass-ceramic and use thereof
EP4745101A1
High-lithium-content glass-ceramic, chemically strengthened glass-ceramic and use thereof
WO2025162193A1
Microcrystalline glass, preparation method therefor and use thereof
WO2025162318A1
Chemically strengthened microcrystalline glass, cover glass, electronic device, and glass device
WO2026067725A1