Nanocrystalline InON film with fast and stable electrochromic response and preparation method and application thereof

Nanocrystalline InON thin films were prepared by DC magnetron sputtering, which solved the problems of slow response and poor stability of inorganic electrochromic materials, and achieved rapid electrochromism and high stability, making them suitable for applications such as smart windows and anti-glare rearview mirrors.

CN118930065APending Publication Date: 2024-11-12XINYU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411044171.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing inorganic electrochromic materials, such as WO3, have long response times and poor stability, which cannot meet the application requirements of smart windows, anti-glare rearview mirrors, and other applications that require instant response.

Method used

Nanocrystalline InON thin films with a thickness of 350–450 nm were prepared by DC magnetron sputtering. By controlling the vacuum level and gas composition of the sputtering chamber and adjusting the oxygen content, a nanocrystalline structure was formed.

Benefits of technology

It achieves short electrochromic response time and good cycle stability, making it suitable for applications requiring instant response and high stability, such as smart windows and automatic anti-glare rearview mirrors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930065A_ABST
    Figure CN118930065A_ABST
Patent Text Reader

Abstract

The invention discloses a nanocrystalline InON film with fast and stable electrochromic response and a preparation method of the nanocrystalline InON film. By controlling the vacuum degree of the sputtering chamber, the oxidation and crystallization of the InON film can be simultaneously realized in the growth process of the InON film, and the oxygen content of the InON film and the electrochromic properties such as optical modulation and response time closely related to the oxygen content can be conveniently adjusted. The film has the characteristic of fast electrochromic response, the shortest fading time is only 0.19 s, and the shortest coloring time is only 0.40 s. Meanwhile, the thin film also has excellent cycling stability and environmental tolerance, and is very suitable for application scenes requiring immediate response and high stability. The direct-current magnetron sputtering method adopted by the invention has the following advantages of high sputtering efficiency, uniform film coating, good film substrate adhesiveness, easiness in large-area preparation, high repeatability, simplicity and easiness in implementation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochromic thin film materials, and in particular relates to a nanocrystalline InON thin film with fast and stable electrochromic response and a preparation method and application thereof. Background Art

[0002] The electrochromic effect refers to the phenomenon that the optical properties of materials, such as reflectivity, transmittance and absorptivity, undergo stable and reversible changes under the action of an external electric field, which is manifested in the reversible changes of color and transparency. This phenomenon was first discovered by Deb in 1969 and applied to electrochromic devices. Many studies have shown that electrochromic devices have potential applications in smart windows, automatic anti-glare rearview mirrors, and spacecraft thermal control and sensors due to their unique advantages.

[0003] Generally, the main indicators for evaluating the electrochromic performance of a material include color change efficiency, response time, cycle stability, etc. Among them, the response time indicates the time required for the material to change from one color state to another. In existing research, WO3 is a typical representative of inorganic electrochromic materials. It has a long response time, usually fading time of more than 5s, and coloring time of more than 10s. Another inorganic electrochromic material that has been studied more is NiO. According to incomplete statistics, the average coloring and fading time of NiO in the literature is about 5.5s. Obviously, for some application scenarios that require instant response or fast switching, such as smart glasses, anti-glare rearview mirrors, etc., this speed level is still far from enough.

[0004] Although inorganic electrochromic materials such as WO3 are generally considered to have good long-term cycle stability and environmental tolerance, there are still some problems and challenges. For example, during multiple electrochromic cycles, the depth and speed of WO3 color change will decrease, and some charges will gradually accumulate inside the material and cannot be completely released; in a high humidity environment, WO3 is prone to hydration reaction to generate hydrated tungsten oxide (WO3·nH2O), which causes structural changes in the material, thereby affecting its electrochromic performance; in addition, long-term redox reactions may cause changes in the WO3 lattice structure, resulting in lattice defects and non-stoichiometric oxides, which in turn affect its stability.

[0005] At present, the main strategies to solve the problems of slow response and poor stability of the above-mentioned electrochromic materials include designing nanostructures and porous structures, optimizing electrodes and electrolytes, material doping and composite material design, and improving processes and preparation methods. However, since the color change mechanism of WO3 is an intervalence transition model, also known as a double injection model, the diffusion rate and path length of ions and electrons inside the material have a direct impact on the response time; at the same time, repeated ion injection and release will cause the volume expansion and structural strain of the material, lattice structure phase change, and charge accumulation in local areas, resulting in a decrease in the efficiency of the electrochromic process and poor stability. Therefore, the above-mentioned optimization measures cannot fundamentally solve the key problems of slow response and poor stability of WO3. Instead, finding a new electrochromic material with fast response and good stability has become the key to solving the problem. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0008] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a nanocrystalline InON film with fast and stable electrochromic response and a preparation method and application thereof.

[0009] To solve the above technical problems, the present invention provides the following technical solution: the InON film has a thickness of 350-450 nm, and has a characteristic peak with low intensity and wide peak shape only at 2θ=32.957°. It has a nanocrystalline structure and is prepared by DC magnetron sputtering.

[0010] Another object of the present invention is to provide a method for preparing a nanocrystalline InON film with fast and stable electrochromic response.

[0011] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:

[0012] Using high-purity In target as target material and ITO conductive glass as substrate, the sputtering chamber is evacuated, and a mixed gas of high-purity Ar and N2 is introduced to perform DC magnetron sputtering to obtain a nanocrystalline InON film with fast and stable electrochromic response.

[0013] As a preferred embodiment of the preparation method of the present invention, the vacuum of the sputtering chamber is 4×10 -4 ~8×10 -4 Pa.

[0014] As a preferred scheme of the preparation method described in the present invention, wherein: the DC magnetron sputtering, wherein the Ar gas flow rate is 8 sccm, the N2 gas flow rate is 12 sccm, the sputtering gas pressure is 0.3-0.8 Pa, the sputtering power is 40-50 W, the substrate temperature is room temperature 20°C, and the sputtering deposition time is 1-1.5 h.

[0015] Another object of the present invention is to provide a nanocrystalline InON film with fast and stable electrochromic response for use in preparing an electrochromic device.

[0016] As a preferred solution of the application of the present invention, the InON film switches its color between gray-brown and light reddish-brown through an electrochromic reaction occurring on its surface.

[0017] As a preferred solution for the application of the present invention, the electrochromic reaction is achieved by applying a DC voltage of ±0.5 to ±1.5 V using an InON film as a working electrode, a Pt sheet as a counter electrode, and a 0.5 mol / L Na2SO4 aqueous solution as an electrolyte.

[0018] As a preferred solution of the application of the present invention, the electrochromic response occurs in the full band of visible light, and its wavelength range is 380 to 780 nm.

[0019] As a preferred solution for the application of the present invention, the electrochromic response is fast, including a fading time of only 0.19 s at the shortest and a coloring time of only 0.40 s at the shortest.

[0020] As a preferred solution of the application of the present invention, the stable InON film means that after 10 to 100 cyclic voltammetry (CV) tests, the CV curve area can still be maintained above 95%.

[0021] Beneficial effects of the present invention:

[0022] (1) The present invention only introduces Ar and N2 during the sputtering deposition process, and adjusts the oxygen concentration in the chamber by precisely controlling the vacuum degree of the chamber. In this environment, the film can be oxidized and crystallized simultaneously during the growth process, thereby forming a nanocrystalline InON film. This not only simplifies the process flow and reduces the demand for gas, but also improves production efficiency and film quality.

[0023] (2) The present invention can conveniently adjust the oxygen content in the nanocrystalline InON film and the electrochromic properties such as optical modulation and response time closely related thereto by controlling the vacuum degree of the chamber. The film has the advantages of ultrafast electrochromic response, good cycle stability and environmental tolerance, and is very suitable for application scenarios that require instant response and high stability.

[0024] (3) The present invention adopts a DC magnetron sputtering method, which has the advantages of high sputtering efficiency, uniform coating, good film-base adhesion, easy large-area preparation, high repeatability, and a simple method that is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0026] Figure 1 The X-ray diffraction (XRD) patterns of the embodiments and comparative examples of the present invention are shown in FIG. Figure 1 (a) is the XRD spectrum of the InON thin films prepared in Examples 1 to 3 and Comparative Examples 1 to 2 of the present invention, Figure 1 (b) is a partial enlarged view.

[0027] Figure 2 is the optical transmittance curve of the nanocrystalline InON film obtained in Examples 1 to 3 of the present invention, wherein: Figure 2 (a) are respectively Embodiment 1 of the present invention, Figure 2 (b) is embodiment 2 of the present invention, Figure 2 (c) is Example 3 of the present invention.

[0028] Figure 3 The chronoamperometric (CA) curves of the nanocrystalline InON films prepared in Examples 1 to 3 of the present invention, wherein: Figure 3 (a) are respectively Embodiment 1 of the present invention, Figure 3 (b) is embodiment 2 of the present invention, Figure 3 (c) is Example 3 of the present invention.

[0029] Figure 4 CV curves of nanocrystalline InON films prepared in Examples 1 to 3 of the present invention, wherein: Figure 4 (a) are respectively Embodiment 1 of the present invention, Figure 4 (b) is embodiment 2 of the present invention, Figure 4 (c) is Example 3 of the present invention. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0032] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0033] The substrate used in the present invention is ITO conductive glass with a size of 25×40×0.7 mm and a resistance of 3.5Ω / sq;

[0034] The high-purity In target used in the present invention has a diameter of 76.2 mm, a thickness of 5 mm, and a purity of 99.999%;

[0035] The purity of the high-purity Ar gas and N2 gas used in the present invention is 99.999%;

[0036] The sputtering coating system used in the present invention is a JGP 500A high vacuum three-target magnetron co-sputtering coating system;

[0037] The ITO conductive glass in the present invention is cleaned according to the following method:

[0038] In an ultrasonic cleaning machine, analytically pure acetone, ethanol, and deionized water with a resistivity of 18.2 MΩ·cm were used for ultrasonic cleaning for 15 minutes each, and the pretreated ITO conductive glass was obtained after drying.

[0039] The film prepared by the present invention is tested and characterized by referring to the following method:

[0040] The microscopic crystal structure of the InON film was determined by powder X-ray diffractometer, with a 2θ measurement range of 15 to 70°;

[0041] The optical transmittance curve of InON film was measured by UV-visible spectrophotometer, and the wavelength measurement range was 300-800nm;

[0042] In the electrochemical workstation, the CA curve and CV curve of the nanocrystalline InON film were measured using a three-electrode system to obtain its electrochromic response time and cycle stability, wherein the working electrode was the prepared nanocrystalline InON film, the counter electrode was a Pt sheet, the reference electrode was an Ag / AgCl electrode, the electrolyte solution was a 0.5 mol / L Na2SO4 aqueous solution, and the applied voltage was ±0.5 to ±1.5 V.

[0043] Example 1

[0044] This embodiment provides a method for preparing a nanocrystalline InON film with fast and stable electrochromic response, specifically:

[0045] In an ultrasonic cleaning machine, analytically pure acetone, ethanol, and deionized water with a resistivity of 18.2 MΩ·cm were used for ultrasonic cleaning for 15 minutes each, and the pretreated ITO conductive glass was obtained after drying.

[0046] High-purity In target was used as sputtering target, pre-treated ITO conductive glass was used as substrate, and the chamber was vacuumed to 4.0×10 -4 Pa, a mixed gas of Ar gas and N2 gas was introduced, wherein the Ar gas flow rate was 8sccm, the N2 gas flow rate was 12sccm, the sputtering pressure was adjusted to 0.8Pa, the sputtering power was 40W, the deposition temperature was room temperature, and the sputtering deposition was performed for 1h to obtain a nanocrystalline InON film with a thickness of about 400nm and an oxygen content of about 2.6%. Its crystal structure, optical modulation, response time and cycle stability were measured. The results are shown in Figure 1 , 2 (a), 3(a), 4(a).

[0047] Example 2

[0048] The difference between this embodiment and embodiment 1 is that the chamber vacuum is evacuated to 6.0×10 -4 Pa, the specific preparation method is:

[0049] High-purity In target was used as the sputtering target, pre-treated ITO conductive glass was used as the substrate, and the chamber was vacuumed to 6.0×10 -4 Pa, a mixed gas of Ar gas and N2 gas was introduced, wherein the Ar gas flow rate was 8sccm, the N2 gas flow rate was 12sccm, the sputtering pressure was adjusted to 0.8Pa, the sputtering power was 40W, the deposition temperature was room temperature, and the sputtering deposition was performed for 1h to obtain a nanocrystalline InON film with a thickness of about 400nm and an oxygen content of about 4.3%. Its crystal structure, optical modulation, response time and cycle stability were measured. The results are shown in Figure 1 , 2 (b), 3(b), and 4(b).

[0050] Example 3

[0051] The difference between this embodiment and embodiment 1 is that the chamber is vacuumed to 8.0×10 -4 Pa, the specific preparation method is:

[0052] High-purity In target was used as the sputtering target, pre-treated ITO conductive glass was used as the substrate, and the chamber was vacuumed to 8.0×10 -4 Pa, a mixed gas of Ar gas and N2 gas was introduced, wherein the Ar gas flow rate was 8sccm, the N2 gas flow rate was 12sccm, the sputtering pressure was adjusted to 0.8Pa, the sputtering power was 40W, the deposition temperature was room temperature, and the sputtering deposition was performed for 1h to obtain a nanocrystalline InON film with a thickness of about 400nm and an oxygen content of about 6.8%. Its crystal structure, optical modulation, response time and cycle stability were measured. The results are shown in Figure 1 , 2 (c), 3(c), and 4(c).

[0053] Comparative Example 1

[0054] The difference between this comparative example and Example 1 is that the chamber is vacuumed to 1×10 -3 Pa, the specific preparation method is:

[0055] High-purity In target was used as the sputtering target, pre-treated ITO conductive glass was used as the substrate, and the chamber was vacuumed to 1.0×10 -3 Pa, a mixed gas of Ar gas and N2 gas was introduced, wherein the Ar gas flow rate was 8sccm, the N2 gas flow rate was 12sccm, the sputtering pressure was adjusted to 0.8Pa, the sputtering power was 40W, the deposition temperature was room temperature, and the sputtering deposition was performed for 1h to obtain an amorphous InON film with a thickness of about 400nm. Its crystal structure was determined. The results are as follows Figure 1 shown.

[0056] Comparative Example 2

[0057] The difference between this comparative example and Example 1 is that the chamber is vacuumed to 2×10 -3 Pa, the specific preparation method is:

[0058] High-purity In target was used as sputtering target, pre-treated ITO conductive glass was used as substrate, and the chamber was vacuumed to 2×10 - 3 Pa, a mixed gas of Ar gas and N2 gas was introduced, wherein the Ar gas flow rate was 8sccm, the N2 gas flow rate was 12sccm, the sputtering pressure was adjusted to 0.8Pa, the sputtering power was 40W, the deposition temperature was room temperature, and the sputtering deposition was performed for 1h to obtain an amorphous InON film with a thickness of about 400nm. Its crystal structure was determined. The results are as follows Figure 1 shown.

[0059] Figure 1 The XRD patterns of InON films prepared under different chamber vacuum conditions are shown. Figure 1 (a) It can be seen that when the chamber vacuum is 10 -3 Pa level (Comparative Examples 1 and 2), except for the diffraction peak of the ITO substrate, no other diffraction peaks appeared, indicating that the InON film has an amorphous structure. -4 At the Pa level (Examples 1, 2, and 3), in addition to the diffraction peak of the ITO substrate, an obvious InON diffraction peak appeared at 2-Theta = 32.957°. This shows that by properly controlling the chamber vacuum, oxidation and crystallization of the InON film can be achieved simultaneously during its growth. The average grain size corresponding to this diffraction peak is calculated to be 16.7 nm using the Scherrer formula. Figure 1 The enlarged image of (b) further shows the diffraction peak in detail. By comparison, it is found that the diffraction peak is located between the InN (101) peak (33.215°, PDF#65-3412) and the In2O3 (110) peak (32.618°, PDF#22-0336). According to Bragg's law, it can be inferred that the interplanar spacing of the InON diffraction peak is slightly larger than the interplanar spacing of InN (101), but smaller than the interplanar spacing of In2O3 (110). This is consistent with the fact that InON is partially oxygen-doped InN, where the introduction of oxygen causes the InON lattice to expand. In addition, many studies have shown that nanoscale grain size can also cause lattice expansion. Therefore, the incorporation of oxygen and the formation of nanocrystals work together to increase the interplanar spacing of InON from Increase to In short, when the chamber vacuum is 10 -4 At the Pa level, the prepared InON films consistently present a nanocrystalline structure.

[0060] like Figure 2 As shown in the figure, compared with the deposited state, the transmittance of InON films in the colored and faded states has changed significantly in the full wavelength range of visible light from 380 to 780 nm. This shows that they exhibit electrochromic response in the entire visible spectrum. In addition, as the chamber pressure increases from 4.0×10 -4 Pa increased to 8.0×10 -4 When Pa, or the oxygen content, increases from 2.6% to 6.8%, the optical modulation (ΔT) of the InON film at 650nm wavelength increases from 15.2% to 27.8%, but both appear as a hue change between gray-brown and light red-brown.

[0061] Figure 3The CA curve in shows the response time of nanocrystalline InON films prepared under different chamber vacuums. As the chamber pressure increases, the fading time of the InON film is almost constant at about 0.20s, but the coloring time gradually decreases from 0.46s to 0.40s. This shows that the electrochromic response of the InON film is closely related to its oxygen content. The resistivity test results show that as the chamber pressure or oxygen content increases, the resistivity of the InON film decreases, so the applied voltage can be more effectively transferred to the electrolyte, thereby accelerating the movement of ions and reducing the response time. Moreover, both times are significantly shorter than the values ​​reported in the literature, indicating that the electrochromic response of the nanocrystalline InON film is very fast. This is because InON is a surface-reactive electrochromic material, and its electrochemical reaction only occurs on the film surface in contact with the electrolyte, and the H involved in the reaction + The ions and OH- do not need to enter the film. Compared with the double-injection electrochromic WO3 film, the common ion diffusion coefficient and diffusion path length limitations are eliminated, allowing the InON film to achieve a very fast electrochromic response.

[0062] like Figure 4 As shown in the figure, the nanocrystalline InON film exhibits excellent cycle stability under different chamber vacuums. After 10 to 100 CV tests, the current density and peak position remain consistent, with only a slight decrease observed, and the CV curve area is almost unchanged, maintaining above 95%. In addition, the colored and faded InON films were exposed to air for several days after power was turned off to study their environmental tolerance and bistability. The optical test results show that their optical transmittance does not change significantly compared with the values ​​measured immediately after the electrochromic switching. This indicates that the InON film can maintain its coloring and fading states for a long time in a real environment. Therefore, the nanocrystalline InON film has excellent cycle stability and environmental tolerance, which will be very beneficial in practical applications. This excellent stability of the nanocrystalline InON film can be attributed to its unique surface reaction type and nanocrystalline structure. First, the surface reaction electrochromic mechanism avoids volume expansion, structural strain, lattice phase change and local charge accumulation caused by repeated ion insertion and release, thereby significantly improving the cycle stability of the InON film. By reducing internal stress and structural changes, this mechanism extends the life of the material and maintains the stability of its electrochromic properties. Secondly, the nanocrystalline structure can improve the mechanical strength and durability of the material. The nanoscale particles provide better structural integrity and stability, reducing stress and cracks that may occur during repeated electrochromic cycles. This structure also helps improve the stability of the material under extreme environmental conditions.

[0063] In summary, the present invention provides a nanocrystalline InON film with fast and stable electrochromic response and a preparation method thereof. By controlling the vacuum degree of the sputtering chamber, the oxygen content in the nanocrystalline InON film and the electrochromic properties such as optical modulation and response time closely related thereto can be conveniently adjusted. The film has the advantages of ultrafast electrochromic response, good cycle stability and environmental tolerance, and is very suitable for application scenarios that require instant response and high stability. The present invention adopts a DC magnetron sputtering method, which has the advantages of high sputtering efficiency, uniform film coating, good film-base adhesion, easy large-area preparation, high repeatability, and a simple method and easy implementation.

[0064] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a nanocrystalline InON film with fast and stable electrochromic response, Features: include, High-purity In target was used as target material, ITO conductive glass was used as substrate, the sputtering chamber was vacuumed, and high-purity Ar and N were introduced. 2 A mixed gas is used for DC magnetron sputtering to obtain a nanocrystalline InON film with fast electrochromic response and stability.

2. The preparation method according to claim 1, Features: The sputtering chamber vacuum is 4×10 -4 ~8×10 - 4 Pa.

3. The preparation method according to claim 1, Features: The DC magnetron sputtering, wherein the Ar gas flow rate is 8 sccm, N 2 The gas flow rate is 12 sccm, the sputtering gas pressure is 0.3-0.8 Pa, the sputtering power is 40-50 W, the substrate temperature is room temperature 20° C., and the sputtering deposition time is 1-1.5 h.

4. A nanocrystalline InON thin film having a fast and stable electrochromic response obtained by the preparation method according to any one of claims 1 to 3, Features: The nanocrystalline InON film has a thickness of 350-450 nm, and has a characteristic peak with relatively low intensity and relatively wide peak shape only at 2θ=32.957°, which is a nanocrystalline structure.

5. Use of the nanocrystalline InON film with fast and stable electrochromic response as claimed in claim 4 in the preparation of electrochromic devices.

6. The use according to claim 5, Features: The InON film switches its color between gray-brown and light reddish-brown through an electrochromic reaction occurring on its surface.

7. The use according to claim 6, Features: The electrochromic reaction uses InON film as the working electrode, Pt sheet as the counter electrode, and 0.5 mol / L Na 2 SO 4 The aqueous solution is an electrolyte, which is achieved by applying a DC voltage of ±0.5 to ±1.5V.

8. The use according to claim 5, Features: The electrochromic response occurs in the entire visible light band, and its wavelength range is 380-780nm.

9. The use according to claim 5, Features: The electrochromic response is fast, including a fading time of only 0.19 s at the shortest and a coloring time of only 0.40 s at the shortest.

10. The use according to claim 5, Features: The stable nanocrystalline InON film means that after 10 to 100 cyclic voltammetry tests, the CV curve area can still be maintained above 95%.

Citation Information

Patent Citations

  • Amorphous WO3 film with rapid electrochromic response effect as well as preparation method and application of amorphous WO3 film

    CN117778972A

  • Method for using sputtering target and method for manufacturing oxide film

    US20140102877A1

  • High Resolution Strain Gages for Ceramic Matrix Composites and Methods of Manufacture Thereof

    US20180003576A1

  • Electronic Device

    US20180011447A1