Modified hybrid fiber and low-carbon anti-crack concrete prepared from same
By modifying hybrid fibers of basalt fiber, ceramic fiber and carbon fiber with starch ether, graphene, acid, silane coupling agent and nanomaterials, and combining it with centrifugal collision process, the problem of insufficient crack resistance and durability of concrete in the existing technology is solved, and the mechanical and durability properties of concrete are improved while reducing the amount of cement used.
Patent Information
- Application Number
- CN202410989058.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing hybrid fiber modification technologies have limited effectiveness in improving the crack resistance and durability of concrete, especially in achieving good mechanical and durability properties while reducing cement usage.
A hybrid fiber, consisting of basalt fiber, ceramic fiber, and carbon fiber, was prepared by pretreatment with starch ether and graphene, acid immersion, modification with silane coupling agent, and modification with nano zinc oxide/nano zirconium carbide, combined with a multi-stage centrifugal collision process. This modified hybrid fiber was then applied to low-carbon crack-resistant concrete.
It significantly improves the tensile strength and durability of concrete, while enhancing its mechanical properties and durability, and significantly improving its crack resistance, all while reducing the amount of cement used.
Smart Images

Figure BDA0004958357550000061 
Figure BDA0004958357550000071 
Figure BDA0004958357550000072
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a modified hybrid fiber and a low-carbon anti-cracking concrete prepared by using the modified hybrid fiber. Background Art
[0002] The durability of concrete is related to the service life of the project, among which the crack resistance of concrete plays a decisive role in the durability of concrete; how to improve the crack resistance of concrete has important practical significance and economic value. The composite of cement-based materials can improve the performance of concrete, among which the use of fiber reinforcement is an effective measure to improve the performance of concrete.
[0003] Fibers used in concrete are mainly divided into two categories according to elastic modulus: one is low elastic modulus fiber, such as polypropylene fiber, polyvinyl alcohol fiber, cellulose fiber, etc.; this type of fiber tends to improve the toughness, impact resistance, thermal burst resistance, etc. of cement concrete; the other is high elastic modulus fiber, such as steel fiber, carbon fiber, etc.; this type of fiber can improve the tensile strength and rigidity of concrete, as well as its toughness. Cement concrete is a multi-phase and multi-component heterogeneous system. Fibers with different properties are mixed and added to concrete, which can be strengthened at different levels, exerting the characteristic effects of different fibers, and the characteristics of different fibers complement each other to achieve a synergistic enhancement effect.
[0004] However, existing mixed fiber or single fiber improvement solutions for the crack resistance of cement concrete usually focus on improving mechanical properties or modifying a single fiber itself, and the corresponding improvement effects are limited. For example, in the document “Study on the Flexural Properties of Fiber-Modified Cement Iron Tailings Sand under Freeze-Thaw Action”, iron tailings sand is modified by fibers and cement, but this scheme mainly focuses on the flexural mechanical properties of fiber-modified tailings sand under freeze-thaw environment; in the document “Surfactant-Modified High-Strength Steel Fiber Concrete and Application Effect”, the steel fiber is surface cleaned and then immersed in a surfactant solution for modification and curing, and then placed in a well-mixed concrete material to obtain a high-strength concrete product. This scheme mainly applies surfactant-modified fibers to concrete to improve the interfacial bonding between the fiber and the matrix, thereby showing good bonding properties; patent application CN116283129 A discloses a composite fiber-modified concrete, in which bamboo fiber and wool fiber are pretreated separately and a coupling agent is added for material composite, and then applied to concrete to improve mechanical strength, flame retardancy and other properties. This scheme mainly combines bamboo fiber, waste wool fiber and nano-silicon dioxide in the form of covalent bonds, but the corresponding mechanical property improvement effect is limited. Summary of the invention
[0005] The main purpose of the present invention is to provide a modified hybrid fiber in view of the problems and shortcomings of the prior art. The hybrid fiber based on basalt fiber, ceramic fiber and carbon fiber is used as a whole. The hybrid fiber is pretreated with starch ether and graphene, soaked in acid, modified with silane coupling agent and modified with nano zinc oxide / nano zirconium carbide, and combined with a fractional centrifugal collision process, the tensile strength of the hybrid fiber can be effectively improved. The hybrid fiber is applied to the preparation of concrete, which can significantly reduce the amount of cement while taking into account good mechanical properties and durability, and is suitable for promotion and application.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a modified hybrid fiber comprises the following steps:
[0008] 1) Mixing basalt fiber, ceramic fiber and carbon fiber to obtain hybrid fiber, adding the hybrid fiber to a starch ether solution for a first soaking treatment, then adding graphene, sequentially performing a first stirring, standing, a second stirring, a second soaking treatment, then alcohol washing, and then drying (80-90° C., 5-6 h) to obtain pretreated hybrid fiber;
[0009] 2) soaking the obtained pretreated mixed fiber in an acid solution, then adding the obtained mixed solution into a planetary ball mill, performing a centrifugal collision, and then washing and drying (100-105° C., 2-3 h);
[0010] 3) adding a silane coupling agent to an alcohol aqueous solution for water bath hydrolysis, then adding the hybrid fiber obtained by the step 2) for heating and stirring; then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution for vacuum infiltration treatment; finally adding the mixture to a planetary ball mill for secondary centrifugal collision to obtain the modified hybrid fiber.
[0011] In the above scheme, the mass ratio of the basalt fiber, the ceramic fiber and the carbon fiber is 1:0.4-0.6:0.4-0.6.
[0012] In the above scheme, the diameter of the basalt fiber is 12-16 μm, the diameter of the ceramic fiber is 2.0-3.0 μm, and the diameter of the carbon fiber is 5-10 μm.
[0013] In the above solution, the length of the mixed fibers is 5 to 8 mm.
[0014] In the above scheme, the concentration of the starch ether solution is 4-6wt%.
[0015] Furthermore, the starch ether has a fineness (100 mesh sieve) of ≥99%, a viscosity (2% aqueous solution) of 1600-2800 mPa·s, and a pH value of 8-12.
[0016] In the above solution, the diameter of the graphene sheet is 1 to 5 μm.
[0017] In the above scheme, the mass ratio of the mixed fiber, starch ether and graphene introduced in step 1) is 1:16-36:0.8-1.2.
[0018] Furthermore, in step 1), the first immersion treatment time is 2 to 3 hours; and the second immersion treatment time is 15 to 18 hours.
[0019] Furthermore, in step 1), the first stirring time is 40 to 60 minutes (60 to 80 r / min rotation speed); the standing time is 2 to 3 hours; and the second stirring time is 30 to 40 minutes (40 to 60 r / min rotation speed, which is lower than the first stirring speed).
[0020] Preferably, the test environment temperature of the entire process in step 1) is 22-26°C.
[0021] In the above scheme, the acid solution can be a nitric acid solution or a sulfuric acid solution.
[0022] Preferably, the acid solution is a nitric acid solution with a concentration of 30-35 vol%.
[0023] In the above scheme, in step 2), the solid-liquid ratio of the introduced pretreated mixed fibers to the acid solution is 1g:100-120ml.
[0024] In the above scheme, the soaking time in step 2) is 30 to 60 minutes.
[0025] In the above scheme, in step 2), the rotation speed of the centrifugal collision is 240-260 r / min (the ball milling beads (zircon) occupy 30-35% of the volume in the tank), and the time is 3-5 hours.
[0026] In the above scheme, in the alcohol aqueous solution, the volume ratio of anhydrous ethanol to water is 7-8:2-3.
[0027] In the above scheme, the amount of the silane coupling agent used is 1.0-1.4% of the mass of the alcohol aqueous solution.
[0028] In the above scheme, the water bath hydrolysis adopts a temperature of 60-65° C. and a time of 20-25 min.
[0029] In the above scheme, in step 3), the mass ratio of the mixed fibers obtained by the treatment in step 2) to the obtained hydrolyzate is 1 to 2:10.
[0030] In the above scheme, in step 3), the temperature used for the heating and stirring treatment is 50-55° C. and the time is 1-1.5 h.
[0031] In the above scheme, in the nano-zinc oxide / nano-zirconium carbide mixed solution, the concentration of nano-zinc oxide is 0.1-0.2 mg / ml, and the concentration of nano-zirconium carbide is 0.2-0.3 mg / ml.
[0032] Furthermore, the particle size of the nano zinc oxide is 20-30 nm, and the particle size of the nano zirconium carbide is 5-20 nm.
[0033] In the above scheme, the vacuum degree used in the vacuum infiltration treatment is 5×10 -2 ~5×10 -3 Pa, time is 2 to 3 hours.
[0034] In the above scheme, the secondary centrifugal collision adopts a rotation speed of 240-260 r / min (the ball milling beads (zircon) occupy 30-35% of the volume in the tank) and a time of 10-20 min.
[0035] The invention also discloses a low-carbon crack-resistant concrete prepared by using the modified hybrid fiber. The modified hybrid fiber is added in the concrete in an amount of 0.15-0.42% of the total mass of the cementitious material.
[0036] Furthermore, in the low-carbon anti-cracking concrete, the components and their weight percentages include: cement 180-190 kg / m 3 , fly ash 85~95kg / m 3 , mineral powder 75~85kg / m 3 , modified hybrid fiber 0.7~1.4kg / m 3 , sand 730~750kg / m 3 , stone 1145~1175kg / m 3 , water 135~145g / m 3 , polycarboxylate water reducer 6.5~7.5kg / m 3 .
[0037] In the above scheme, the cement can be silicate cement with PO 42.5 or above; the fly ash can be F·Ⅲ or F·Ⅱ fly ash with a fineness of 32-38%; the mineral powder can be S75 or above with a specific surface area of 380-400m 2 / kg; the sand is coarse sand, with a fineness modulus of 3.2-3.5, a moisture content of 2.2-2.6%, and a mud content of 1.0-1.2%; the stone is 5-20 mm crushed stone, with a mud content of 0.4-0.6%, a crushing index of 2-4%, and an apparent density of 2650-2700 kg / m 3; The solid content of polycarboxylic acid water-reducing agent is 12.00-13.00%, and the water reduction rate is 26-28%.
[0038] The low-carbon crack-resistant concrete prepared according to the above scheme has a 28d compressive strength of 52-54MPa, which is 35-45kg less than the cement dosage of the same grade of traditional concrete, and the compressive strength at the same age is increased by about 5-8%; the frost resistance grade can reach above F250, the 28d electrical flux is 300-500C, and the 56d electrical flux is 100-200C, and the early anti-cracking performance is improved by more than 20% compared with the same grade of traditional concrete.
[0039] The principle of the present invention is:
[0040] 1) The present invention first mixes three kinds of fibers, namely basalt fiber, ceramic fiber and carbon fiber, and then performs synchronous and comprehensive modification on the obtained hybrid fiber as a whole, so as to effectively ensure the stability of the three kinds of fibers after mixing and the good coordination improvement effect: in the process of hybrid fiber modification, starch ether solution mixed with graphene conductive agent is used for immersion treatment, which can play a role of surface activation while washing impurities on the fiber surface and accelerating the dispersion speed; in addition, the graphene conductive agent (usually containing a small amount of functional groups and having a small sheet diameter and excellent dispersibility in starch ether solution) introduced during the immersion process can show good dispersibility and stability in the starch ether solution (due to the surface activity of the starch ether solution), effectively promote the overall dispersion of the hybrid fiber, and can further promote the graphitization of part of the carbon fiber (the elemental carbon in the graphene is attached to the carbon fiber), which is beneficial to the improvement of the durability of the concrete by the modified fiber in the later stage.
[0041] 2) In the improvement process of the hybrid fibers described in the present invention, a planetary ball milling process based on the centrifugal collision method is further adopted, which mainly utilizes the repeated high-speed rotation and collision of particles under the action of centrifugal collision to generate mechanical energy, thereby promoting the secondary reaction of the modification reaction of the mixed fibers in the starch ether solution and the graphene conductive agent in step 1), thereby ensuring the improvement effect and being simple to operate. At the same time, the structural distribution state of the hybrid fibers can be further improved, which is beneficial to ensuring the dispersion effect of the modified hybrid fibers in concrete.
[0042] 3) The present invention innovatively uses nano zinc oxide and nano zirconium carbide materials to further modify the hybrid fiber, wherein the introduced nano zinc oxide is beneficial to improving the toughness and ductility of the ceramic fiber, and the nano zirconium oxide is beneficial to improving the durability of the hybrid fiber, etc.; nano zinc oxide has good dispersibility and compatibility in the solution system of the present invention, and at the same time, by adjusting the particle size and ratio of nano zinc oxide and nano zirconium carbide, and using a coupling agent to graft and modify the surface of the hybrid fiber under constant temperature heating and stirring conditions, the surface polarity of the hybrid fiber is increased without damaging the hybrid fiber; after the surface modification treatment, a favorable environment is provided for the surface reaction of the hybrid fiber, which is convenient for fiber bonding and additional reactions of other material properties, and promotes the enhancement of its mechanical properties and durability, etc.; finally, it is further combined with a secondary centrifugal collision process to further provide mechanical energy for the nano material modification process and enhance the dispersion effect in the reaction process.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] 1) The present invention adopts a hybrid fiber based on basalt fiber, ceramic fiber and carbon fiber as a whole, firstly pre-treated with starch ether and graphene, acid soaking, silane coupling agent modification and nano zinc oxide / nano zirconium carbide modification, and combined with a fractional centrifugal collision process, which can effectively improve the comprehensive performance of the hybrid fiber (having good tensile strength, etc.);
[0045] 2) The modified hybrid fiber of the present invention is applied to prepare concrete, which can significantly reduce the amount of cement while taking into account good mechanical properties and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a cross-sectional scanning electron microscope image of the low-carbon crack-resistant concrete obtained in Example 1 (magnified 20,000 times).
[0047] Figure 2 This is a cross-sectional scanning electron microscope image of the low-carbon crack-resistant concrete obtained in Example 1 (magnified 3000 times). DETAILED DESCRIPTION
[0048] The present invention is further described in detail below through a specific implementation case. This implementation case is specifically implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given, but the scope of protection of the present invention is not limited to the implementation case given below.
[0049] In the following examples and comparative examples, the cement used is Qingsong PO 42.5R cement; the fly ash is F·III fly ash from Honger Power Plant, with a fineness of 35%; the mineral powder is Baoxin Shengyuan S75 mineral powder, with a specific surface area of 395m 2 / kg; the sand is coarse sand provided by Xinjiang Hetongyuan Building Materials Co., Ltd., with a fineness modulus of 3.4, a moisture content of 2.5%, and a mud content of 1.1%; the stone is crushed stone with a particle size of 5-20 mm, a mud content of 0.4%, a crushing index of 3%, and an apparent density of 2670kg / m 3 The water reducer is a polycarboxylic acid high-performance water reducer provided by Kehuida Chemical Building Materials Co., Ltd., with a solid content of 12.15% and a water reduction rate of 27%;
[0050] Basalt fiber is produced by Tai'an Anfeng New Material Technology Co., Ltd., with a length of 10-14 mm, a diameter of 12-16 μm, and a density of 2.60-2.70 g / cm 3 , tensile strength 3200 ~ 4500MPa, elastic modulus 95 ~ 115GPa; ceramic fiber is produced by Lingshou County Keying New Materials Co., Ltd., length 100 ~ 200mm, diameter 2.0 ~ 3.0μm, density 2.5 ~ 2.70g / cm 3 , tensile strength 2300~2500MPa; carbon fiber is produced by Dongguan Angyu Carbon Fiber Co., Ltd., with a length of 10~15mm, a diameter of 5~10μm, and a density of 1.70~1.80g / cm 3 , tensile strength 3500-3800 MPa, elastic modulus 220-250 GPa. Before use, the basalt fiber, ceramic fiber and carbon fiber are sheared to control the fiber length to 5-8 mm.
[0051] The starch ether was produced by Shanghai Kaiyin Chemical Co., Ltd., with a fineness (100 mesh sieve) ≥99%, a viscosity (2% aqueous solution) of 1600-2800 mPa·s, and a pH value of 8-12; the graphene conductive agent was a graphene dispersion produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., in which the graphene sheet diameter was 1-5 μm and the mass percentage of graphene was 5.0 ωt%; the nano zinc oxide was produced by Bohuas Nanotechnology (Ningbo) Co., Ltd., with a zinc oxide content ≥99.6%, an average particle size of 20-30 nm, and a specific surface area of 30-90 m 2 / g; Nano zirconium carbide is produced by Bohuasi Nanotechnology (Ningbo) Co., Ltd., with a particle size of 5-10nm and 10-20nm mixed in a 1:1 mass ratio, melting point 3530-3550℃, purity>99.9%, density 6.70-6.75g / cm 3 Specific surface area: 52~56m 2 / g.
[0052] In the following examples, in the centrifugal collision step, the volume percentage of zircon in the tank is 30%.
[0053] Example 1
[0054] A method for preparing a modified hybrid fiber comprises the following steps:
[0055] 1) Basalt fiber, ceramic fiber and carbon fiber are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain a hybrid fiber; 1 part (by weight, the same below) of the hybrid fiber is added to 400 parts of a 4wt% starch ether solution for immersion treatment for 2 hours, and then 0.8 parts of a graphene conductive agent are added, and the mixture is uniformly stirred at a speed of 60r / min for 60 minutes under an experimental environment temperature of 24°C, and after standing for 2 hours, it is uniformly stirred at a speed of 60r / min for 30 minutes, and after standing and soaking for 15 hours, it is washed with alcohol (anhydrous ethanol), and then dried at 80°C for 6 hours to perform a degumming treatment;
[0056] 2) Soaking the mixed fibers preliminarily treated in step 1) in a 30% nitric acid solution at a solid-liquid ratio of 1 g:100 ml for 30 minutes, then adding the resulting mixed solution into a planetary ball mill, performing a centrifugal collision (at a speed of 240 r / min for 3 hours), then washing with water, and drying at 100° C. for 2 hours;
[0057] 3) adding a silane coupling agent (in an amount of 1.0 wt% of the alcohol aqueous solution) to an alcohol aqueous solution (the volume ratio of ethanol to water is 7:3), and hydrolyzing the mixture in a water bath at 60° C. for 20 min, and then adding the mixed fibers treated in step 2) at a mass ratio of 1:10 between the mixed fibers and the obtained hydrolyzate, and heating and stirring the mixture at 50° C. for 1 h; and then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution (the concentration of nano zinc oxide is 0.1 mg / ml, and the concentration of nano zirconium carbide is 0.2 mg / ml) at 5×10 -2 The mixture was subjected to vacuum infiltration treatment for 2 h at a vacuum degree of Pa; finally, the mixture was added to a ball mill for secondary centrifugal collision (at a speed of 240 r / min for 10 min), thereby obtaining the modified hybrid fiber (referred to as hybrid 1).
[0058] The modified hybrid fiber prepared in this embodiment has an average fiber length of 6 mm and a density of 2.45 g / cm 3 The tensile strength is 6500MPa, which is significantly improved compared with the tensile strength of a single fiber (the highest tensile strength among the three fibers, the same below).
[0059] Figure 1 and Figure 2 The cross-sectional scanning electron microscope images at different magnifications of the low-carbon anti-cracking concrete obtained in Example 1 show that the mixed fibers are evenly distributed, and the hydration products are attached to the fiber surface, which fills the interface transition zone well, which is beneficial to increase the bonding force between the mortar and the aggregate, and the concrete structure is dense.
[0060] Application Example 1
[0061] The modified hybrid fiber obtained in Example 1 is applied to prepare low-carbon crack-resistant concrete (C40 grade), and the specific steps include:
[0062] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 1, and the performance test results of the obtained concrete are shown in Table 2.
[0063] Table 1 Concrete mix ratio (kg / m 3 )
[0064] Group cement Fly ash Mineral powder sand stone water Water reducing agent Modified hybrid fiber Benchmarks 225 90 80 720 1125 155 8.5 Application Example 1 185 90 80 740 1160 140 7.0 1.0 (Misc 1)
[0065] Table 2 Performance test results of concrete obtained in Application Example 1
[0066]
[0067] The above results show that the modified hybrid fiber low-carbon crack-resistant concrete obtained in this application example can improve the mechanical properties and durability of concrete and ensure good working performance when the proportion of cement is reduced by 40kg, compared with the concrete of the same grade benchmark group. Among them, the improvement effects of mechanical properties and durability are as follows: in terms of mechanical properties, the 28d compressive strength is increased by 13% and the flexural strength is increased by 64% compared with the benchmark group; in terms of durability, the 28d and 56d electric fluxes are reduced by 578C and 558C respectively compared with the benchmark group, and the 56d electric flux can reach below 200C, the antifreeze grade can reach F250, and the effective antifreeze-thaw cycle is increased by 100 times compared with the benchmark. In terms of early crack resistance, the crack area is reduced by 18% compared with the benchmark.
[0068] Example 2
[0069] A method for preparing a modified hybrid fiber comprises the following steps:
[0070] 1) Basalt fiber, ceramic fiber and carbon fiber are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain 1 part of mixed fiber, which is added to 500 parts of a 5% starch ether solution for immersion treatment for 3 hours, and then 1.0 parts of a graphene conductive agent is added, and the mixture is uniformly stirred at a speed of 60 r / min for 80 minutes under an experimental environment temperature of 24°C, and then allowed to stand for 2 hours, and then uniformly stirred at a speed of 60 r / min for 30 minutes, and then allowed to stand and soak for 15 hours, and then washed with alcohol (anhydrous ethanol), and then dried at 80°C for 6 hours to perform a degumming treatment;
[0071] 2) Soaking the mixed fibers preliminarily treated in step 1) in a 35% nitric acid solution at a solid-liquid ratio of 1 g:120 ml for 30 min, then adding the resulting mixed solution into a planetary ball mill, performing a centrifugal collision (at a speed of 240 r / min for 3 h), then washing with water, and drying at 100° C. for 2 h;
[0072] 3) adding a silane coupling agent (1.2 wt% of the alcohol aqueous solution) to an alcohol aqueous solution (the volume ratio of ethanol to water is 8:2), and hydrolyzing the mixed fibers in a water bath at 60° C. for 20 min, and then adding the mixed fibers obtained by the treatment in step 2) at a mass ratio of 1:10 between the mixed fibers and the obtained hydrolyzate, and heating and stirring the mixed fibers at 50° C. for 1 h; and then immersing the mixed fibers in a nano zinc oxide / nano zirconium carbide mixed solution (the concentration of nano zinc oxide is 0.1 mg / ml, and the concentration of nano zirconium carbide is 0.2 mg / ml) at 5×10 -3 The mixture was subjected to vacuum infiltration treatment at a vacuum degree of Pa for 2 hours; finally, the mixture was added to a ball mill for secondary centrifugal collision, i.e., the mixture was subjected to a rotation speed of 240 r / min for 10 minutes, thereby obtaining the modified hybrid fiber (referred to as Hybrid 2).
[0073] The modified hybrid fiber prepared in this embodiment has an average fiber length of 6 mm and a density of 2.46 g / cm 3 The tensile strength is 6650MPa, which is significantly improved compared with the tensile strength of a single fiber.
[0074] Application Example 2
[0075] The modified hybrid fiber obtained in Example 2 is applied to prepare low-carbon crack-resistant concrete (C40 grade), and the specific steps include:
[0076] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 3, and the performance test results of the obtained concrete are shown in Table 4.
[0077] Table 3 Concrete mix ratio (kg / m 3 )
[0078]
[0079] Table 4 Performance test results of concrete obtained in Application Example 2
[0080]
[0081] The above results show that the modified hybrid fiber low-carbon anti-cracking concrete obtained in this application example can simultaneously improve the mechanical properties and durability of concrete compared with the same grade benchmark group concrete under the condition of reducing the mix ratio of 40kg cement. Specifically, in terms of mechanical properties, the 28d compressive strength is increased by 20% and the flexural strength is increased by 73% compared with the benchmark group. In terms of durability, the 28d and 56d electric fluxes are reduced by 592C and 594C respectively compared with the benchmark group, and the 56d electric flux can reach below 150C, with excellent performance. The frost resistance grade in this application example can reach F250, which is 100 times higher than the benchmark in effective freeze-thaw resistance. In terms of early crack resistance, the crack area is reduced by 23% compared with the benchmark.
[0082] Comparative Example 1
[0083] A method for preparing a modified hybrid fiber comprises the following steps:
[0084] 1) Basalt fiber, ceramic fiber and carbon fiber are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain a mixed fiber; 1 part of the mixed fiber is added to 400 parts of a 4% acetone solution for immersion for 2 hours, stirred uniformly at a speed of 60 r / min for 60 minutes under an experimental environment temperature of 24°C, allowed to stand for 2 hours, stirred uniformly at a speed of 60 r / min for 30 minutes, allowed to stand and soak for 15 hours, then washed with alcohol (anhydrous ethanol), and then dried at 80°C for 6 hours to perform a degumming treatment;
[0085] 2) soaking the mixed fibers after the preliminary treatment in step 1) in a 30% nitric acid solution with a solid-liquid ratio of 1g:100ml for 30 minutes, then adding the resulting mixed solution into a planetary ball mill, performing a centrifugal collision at a speed of 240r / min for 3 hours, then washing with water, and drying at 100°C for 2 hours;
[0086] 3) adding a silane coupling agent at a mass ratio of 1.0% to an alcohol aqueous solution (the volume ratio of ethanol to water is 7:3), hydrolyzing the mixture in a water bath at 60° C. for 20 min, then adding the mixed fibers treated in step 2) at a mass ratio of 1:10 between the mixed fibers and the obtained hydrolyzate, and heating and stirring the mixture at 50° C. for 1 h; then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution (the concentration of nano zinc oxide is 0.1 mg / ml, and the concentration of nano zirconium carbide is 0.2 mg / ml) at 5×10 -2 The mixture was subjected to vacuum infiltration treatment for 2 h at a vacuum degree of Pa; finally, the mixture was added to a ball mill for secondary centrifugal collision, i.e., the mixture was subjected to a rotation speed of 240 r / min for 10 min, thereby obtaining the modified hybrid fiber (referred to as hybrid 3).
[0087] The modified hybrid fiber prepared in this comparative example has a fiber length of 6 mm and a density of 2.60 g / cm 3 The tensile strength is 3200MPa, which is basically unchanged compared with the tensile strength of a single fiber.
[0088] The modified hybrid fiber obtained in this comparative example is applied to prepare low-carbon anti-cracking concrete (C40 grade), and the specific steps include:
[0089] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 5, and the performance test results of the obtained concrete are shown in Table 6.
[0090] Table 5 Concrete mix ratio (kg / m 3 )
[0091] Group cement Fly ash Mineral powder sand stone water Water reducing agent Modified hybrid fiber Benchmarks 225 90 80 720 1125 155 8.5 Application Example 3 185 90 80 740 1160 140 7.0 1.0 (Misc 3)
[0092] Table 6 Performance test results of concrete obtained in Application Example 3
[0093]
[0094]
[0095] The above results show that the modified hybrid fiber low-carbon anti-cracking concrete obtained in this application example cannot achieve the simultaneous improvement of the mechanical properties and durability of the concrete under the condition of reducing the mix ratio of 40kg cement compared with the concrete of the same grade benchmark group. Specifically, in terms of mechanical properties, the 28d compressive strength is 13% lower than that of the benchmark group, and the flexural strength is 12% higher than that of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are basically unchanged compared with the benchmark group, and the frost resistance grade is F150 the same as the benchmark group. In terms of early anti-cracking performance, there is no obvious change or even a slight decrease compared with the benchmark group. It is impossible to ensure the mechanical properties and durability of the obtained concrete under the premise of reducing the cement dosage.
[0096] Comparative Example 2
[0097] A method for preparing a modified hybrid fiber comprises the following steps:
[0098] 1) Basalt fiber, ceramic fiber, and carbon fiber (parameters as described above) are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain a hybrid fiber; 1 part of the hybrid fiber is added to 400 parts of a 4% starch ether solution for immersion treatment for 2 hours, and then 0.8 parts of a graphene conductive agent are added, and the mixture is uniformly stirred at a speed of 60 r / min for 60 minutes under an experimental environment temperature of 24° C., and then allowed to stand for 2 hours, and then uniformly stirred at a speed of 60 r / min for 30 minutes, and then allowed to stand and soak for 15 hours, and then washed with alcohol (anhydrous ethanol), and then dried at 80° C. for 6 hours to perform a degumming treatment;
[0099] 2) soaking the mixed fibers after the preliminary treatment in step 1) in a 30% by volume nitric acid solution at a solid-liquid ratio of 1g:100ml for 30 minutes, then washing with water, and drying at 100°C for 2 hours;
[0100] 3) adding 1.0% silane coupling agent to an alcohol aqueous solution (volume ratio of ethanol to water is 7:3) at a mass ratio, hydrolyzing at 60°C for 20 min in a water bath, then adding the mixed fiber obtained by step 2) at a mass ratio of 1:10 to the obtained hydrolyzate, and heating and stirring at 50°C for 1 h; then immersing the obtained mixture in a nano-silicon dioxide solution (concentration of 0.2 mg / ml) at 5×10 -2 The vacuum infiltration treatment was carried out at a vacuum degree of Pa for 2 hours to obtain the modified hybrid fiber (referred to as Hybrid 4).
[0101] The modified hybrid fiber prepared in this comparative example has a fiber length of 6 mm and a density of 2.65 g / cm 3 The tensile strength is 3500MPa, which has no significant change compared with the tensile strength of a single fiber.
[0102] The modified hybrid fiber obtained in this comparative example is used to prepare low-carbon crack-resistant concrete (C40 grade), mainly using the same amount of cement as the reference group and reducing it by 40kg / m 3 There are two application examples of cement dosage (Application Examples 4 and 5 respectively), and the specific steps include:
[0103] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 7, and the performance test results of the obtained concrete are shown in Table 8.
[0104] Table 7 Concrete mix ratio (kg / m 3 )
[0105]
[0106]
[0107] Table 8 Performance test results of concrete obtained in application examples 4 and 5
[0108]
[0109] The above results show that the modified hybrid fiber low-carbon anti-cracking concrete obtained in Application Example 4 has no significant improvement in mechanical properties and durability compared with the same grade benchmark concrete under the same cement ratio. Specifically, in terms of mechanical properties, the 28d compressive strength and flexural strength are basically the same as those of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are 90C and 38C lower than those of the benchmark group, respectively. The frost resistance grade is F150, which is the same as the benchmark group. In terms of early crack resistance, the crack area is 4% lower than that of the benchmark. Compared with the same grade benchmark concrete, the modified hybrid fiber low-carbon anti-cracking concrete obtained in Application Example 5 has no significant improvement in mechanical properties and durability. Specifically, in terms of mechanical properties, the 28d compressive strength and flexural strength are basically the same as those of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are 90C and 38C lower than those of the benchmark group, respectively. The frost resistance grade is F150, which is the same as the benchmark group. In terms of early crack resistance, the crack area is 4% lower than that of the benchmark. Under the condition of reducing the mix ratio of 40kg cement, there is no obvious improvement in the mechanical properties and durability of concrete, and even slightly decreases. Specifically, in terms of mechanical properties, the 28d compressive strength is 10% lower than that of the benchmark group, and the flexural strength is 4% higher than that of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are 42C and 18C lower than those of the benchmark group, respectively. The frost resistance grade is F150, which is the same grade as the benchmark group. In terms of early crack resistance, there is no obvious change in the crack area compared with the benchmark. Under the same cement content ratio, the concrete performance is not much different from that of the benchmark group. Under the condition of reducing the cement content ratio, the concrete performance is slightly lower than that of the benchmark group in some properties.
[0110] Comparative Example 3
[0111] A method for preparing a modified hybrid fiber comprises the following steps:
[0112] 1) Basalt fiber, ceramic fiber and carbon fiber are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain a hybrid fiber; 1 part (by weight, the same below) of the hybrid fiber is added to 400 parts of a 4% starch ether solution for immersion for 2 hours, and then 0.8 parts of a graphene conductive agent is added, and the mixture is uniformly stirred at a speed of 60 r / min for 60 minutes under an experimental environment temperature of 24° C., and then washed with alcohol (absolute ethanol), and then dried at 80° C. for 6 hours to perform a degumming treatment;
[0113] 2) Soaking the mixed fibers preliminarily treated in step 1) in a 30% nitric acid solution at a solid-liquid ratio of 1 g:100 ml for 30 minutes, then adding the resulting mixed solution into a planetary ball mill, performing a centrifugal collision (at a speed of 240 r / min for 3 hours), then washing with water, and drying at 100° C. for 2 hours;
[0114] 3) adding a silane coupling agent at a mass ratio of 1.0% to an alcohol aqueous solution (the volume ratio of ethanol to water is 7:3), hydrolyzing the mixture in a water bath at 60° C. for 20 min, then adding the mixed fibers treated in step 2) at a mass ratio of 1:10 between the mixed fibers and the obtained hydrolyzate, and heating and stirring the mixture at 50° C. for 1 h; then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution (the concentration of nano zinc oxide is 0.1 mg / ml, and the concentration of nano zirconium carbide is 0.2 mg / ml) at 5×10 -2 The mixture was subjected to vacuum infiltration treatment for 2 h at a vacuum degree of Pa; finally, the mixture was added to a ball mill for secondary centrifugal collision (at a speed of 240 r / min for 10 min), thereby obtaining the modified hybrid fiber (referred to as Hybrid 5).
[0115] The modified hybrid fiber prepared in this embodiment has a fiber length of 6 mm and a density of 2.50 g / cm 3 The tensile strength is 3800MPa, which is not significantly improved compared with the tensile strength of a single fiber.
[0116] The modified hybrid fiber obtained in this comparative example is applied to prepare low-carbon anti-cracking concrete (C40 grade), and the specific steps include:
[0117] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 9, and the performance test results of the obtained concrete are shown in Table 10.
[0118] Table 9 Concrete mix ratio (kg / m 3 )
[0119] Group cement Fly ash Mineral powder sand stone water Water reducing agent Modified hybrid fiber Benchmarks 225 90 80 720 1125 155 8.5 Application Example 6 185 90 80 740 1160 140 7.0 1.0 (Misc 5)
[0120] Table 10 Performance test results of concrete obtained in Application Example 6
[0121]
[0122] The above results show that the modified hybrid fiber low-carbon anti-cracking concrete obtained in this application example cannot achieve the simultaneous improvement of the mechanical properties and durability of the concrete when the mix ratio of cement is reduced by 40kg compared with the benchmark group concrete of the same grade. The details are as follows: in terms of mechanical properties, the 28d compressive strength is 11% lower than that of the benchmark group, and the flexural strength is 10% higher than that of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are 43C and 12C lower than that of the benchmark group, respectively, and the performance changes are not obvious. The frost resistance grade is F150, which is at the same level as the benchmark group. In terms of early crack resistance, there is no obvious decrease in the crack area compared with the benchmark.
[0123] Comparative Example 4
[0124] A method for preparing a modified hybrid fiber comprises the following steps:
[0125] 1) Basalt fiber, ceramic fiber and carbon fiber are mixed in a mass ratio of 2:1:1 and trimmed to an average fiber length of 6 mm to obtain a hybrid fiber; 1 part (by weight, the same below) of the hybrid fiber is added to 400 parts of a 4% starch ether solution for immersion treatment for 2 hours, and then 0.8 parts of a graphene conductive agent are added, and the mixture is uniformly stirred at a speed of 60 r / min for 60 minutes under an experimental environment temperature of 24°C, and after standing for 2 hours, it is uniformly stirred at a speed of 60 r / min for 30 minutes, and after standing and soaking for 15 hours, it is washed with alcohol (anhydrous ethanol), and then dried at 80°C for 6 hours to perform a degumming treatment;
[0126] 2) Soaking the mixed fibers after the preliminary treatment in step 1) in a 30% nitric acid solution with a solid-liquid ratio of 1g:100ml for 30 minutes, then adding the resulting mixed solution into a steel forging ball mill, performing a rotation dispersion treatment (at a speed of 80r / min for 3 hours), then washing with water, and drying at 100°C for 2 hours;
[0127] 3) adding a silane coupling agent at a mass ratio of 1.0% to an alcohol aqueous solution (the volume ratio of ethanol to water is 7:3), hydrolyzing the mixture in a water bath at 60° C. for 20 min, then adding the mixed fibers treated in step 2) at a mass ratio of 1:10 between the mixed fibers and the obtained hydrolyzate, and heating and stirring the mixture at 50° C. for 1 h; then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution (the concentration of nano zinc oxide is 0.1 mg / ml, and the concentration of nano zirconium carbide is 0.2 mg / ml) at 5×10 -2 The mixture was subjected to vacuum infiltration treatment at a vacuum degree of Pa for 2 hours; finally, the mixture was added to a steel forging ball mill for secondary rotation dispersion (at a rotation speed of 80 r / min for 10 minutes) to obtain the modified hybrid fiber (referred to as Hybrid 6).
[0128] The modified hybrid fiber prepared in this embodiment has a fiber length of 6 mm and a density of 2.52 g / cm 3 The tensile strength is 3850MPa, which has no significant change compared with the tensile strength of a single fiber.
[0129] The modified hybrid fiber obtained in Example 1 is applied to prepare low-carbon crack-resistant concrete (C40 grade), and the specific steps include:
[0130] First, add coarse and fine aggregates into the mixer and stir evenly for 20 seconds, then dry-mix the cementitious material in the mixer for 30 seconds, then add 1 / 2 of the designed amount of modified hybrid fiber and stir for 30 seconds, then pour water and the remaining 1 / 2 of the designed amount of modified hybrid fiber into the mixer and stir thoroughly for 5 minutes, and control the slump of concrete to (180±20) mm by adjusting the amount of water reducer; the specific mix ratio is shown in Table 11, and the performance test results of the obtained concrete are shown in Table 12.
[0131] Table 11 Concrete mix ratio (kg / m 3 )
[0132] Group cement Fly ash Mineral powder sand stone water Water reducing agent Modified hybrid fiber Benchmarks 225 90 80 720 1125 155 8.5 Application Example 1 185 90 80 740 1160 140 7.0 1.0 (Misc 6)
[0133] Table 12 Performance test results of concrete obtained in Application Example 7
[0134]
[0135] The above results show that the modified hybrid fiber low-carbon anti-cracking concrete obtained in this application example cannot achieve the simultaneous improvement of the mechanical properties and durability of the concrete when the mix ratio of cement is reduced by 40kg compared with the concrete of the same grade benchmark group. Specifically, in terms of mechanical properties, the 28d compressive strength is 13% lower than that of the benchmark group, and the flexural strength is 8% higher than that of the benchmark group. In terms of durability, the 28d and 56d electric fluxes are 16C and 5C lower than that of the benchmark group, respectively, with basically no change. The frost resistance grade is F150, which is the same level as the benchmark group. In terms of early anti-cracking performance, there is no obvious change or even a slight decrease compared with the benchmark group.
[0136] For those skilled in the art, it is easy to improve and modify the present invention without departing from the technology of the present invention, and these improvements and modifications also fall within the scope of protection of the present invention. The present invention is not limited to the above-mentioned embodiments, and any changes within the claims of the present invention are covered within the scope of protection.
Claims
1. A method for preparing a modified hybrid fiber, characterized in that: The following steps are involved: 1) Mixing basalt fiber, ceramic fiber and carbon fiber to obtain hybrid fiber, adding the hybrid fiber to a starch ether solution for a first soaking treatment, then adding graphene, sequentially performing a first stirring, standing, a second stirring, a second soaking treatment, and then washing with alcohol and drying to obtain pretreated hybrid fiber; 2) soaking the obtained pretreated mixed fiber in an acid solution, then adding the obtained mixed solution to perform a centrifugal collision, and then washing with water and drying; 3) adding a silane coupling agent to an alcohol aqueous solution, hydrolyzing it in a water bath, then adding the hybrid fiber obtained by the treatment in step 2), and heating and stirring the fiber; then immersing the obtained mixture in a nano zinc oxide / nano zirconium carbide mixed solution, and performing a vacuum infiltration treatment; and finally performing a secondary centrifugal collision to obtain the modified hybrid fiber.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the basalt fiber, the ceramic fiber and the carbon fiber is 1:0.4-0.6:0.4-0.
6.
3. The preparation method according to claim 1, characterized in that: The diameter of the basalt fiber is 12-16 μm, the diameter of the ceramic fiber is 2.0-3.0 μm, the diameter of the carbon fiber is 5-10 μm; and the length of the mixed fiber is 5-8 mm.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the mixed fiber, starch ether and graphene introduced in step 1) is 1:16-36:0.8-1.
2.
5. The preparation method according to claim 1, characterized in that: In the nano zinc oxide / nano zirconium carbide mixed solution, the concentration of nano zinc oxide is 0.1-0.2 mg / ml, and the concentration of nano zirconium carbide is 0.2-0.3 mg / ml.
6. The preparation method according to claim 1, characterized in that: The first centrifugal collision and the second centrifugal collision both use planetary ball mills; the first centrifugal collision uses a rotation speed of 240-260 r / min for 3-5 hours; the second centrifugal collision uses a rotation speed of 240-260 r / min for 10-20 minutes.
7. The modified hybrid fiber prepared by the preparation method according to any one of claims 1 to 6.
8. A low-carbon crack-resistant concrete prepared by using the modified hybrid fiber according to claim 7, characterized in that: The modified hybrid fiber is added in an amount of 0.15-0.42% of the total mass of the cementitious material in the concrete.
9. The low-carbon crack-resistant concrete according to claim 8, characterized in that: The components and their weight percentages include: cement 180-190 kg / m 3 , fly ash 85~95kg / m 3 , mineral powder 75~85kg / m 3 , modified hybrid fiber 0.7~1.4kg / m 3 , sand 730~750kg / m 3 , stone 1145~1175kg / m 3 , water 135~145g / m 3 , polycarboxylate water reducer 6.5~7.5kg / m 3 .
10. The low-carbon crack-resistant concrete according to claim 8, characterized in that: The sand is coarse sand with a fineness modulus of 3.2-3.5, a moisture content of 2.2-2.6%, and a mud content of 1.0-1.2%; the stone is 5-20 mm crushed stone with a mud content of 0.4-0.6%, a crushing index of 2-4%, and an apparent density of 2650-2700 kg / m 3 .
Citation Information
Cited By
Modified ceramic material based on nano-zinc oxide and preparation method thereof
CN121063911A