Method for improving performance of asphalt mixture by using waste circuit board
By using the non-metallic components of the used circuit board as a modifier and mixing them with asphalt after treatment, the problems of high temperature and insufficient water stability of the asphalt mixture are solved, the performance of the asphalt mixture is improved and the cost is reduced, and environmental protection is achieved. Economic construction effect.
Patent Information
- Application Number
- CN202410988459.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional hot-mixed asphalt mixtures are insufficient in high temperature and water stability, and are prone to ruts and cracks. Modifiers such as SBS are difficult to process, costly and have serious pollution emissions.
The non-metallic components of the used circuit board are used as the modifier, and then mixed with asphalt through crushing, screening and soaking of silane coupling agent to form a modified asphalt mixture, which improves its high temperature stability and water loss resistance.
It significantly improves the high temperature stability and water loss resistance of asphalt mixture, reduces production and construction costs, and takes into account environmental protection and economicality.
Smart Images

Figure CN118930132A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of asphalt pavement, in particular to a method for improving the performance of asphalt mixture by utilizing waste circuit boards. Background Art
[0002] Asphalt pavement has the advantages of smooth surface, no joints, comfortable driving, low vibration, low noise, wear resistance, no dust, easy cleaning, short construction period, simple maintenance and repair, and recyclable use. Therefore, it has accounted for more than 90% of the high-grade highway applications. In order to build a strong transportation country, a large number of highway asphalt pavements are under new construction and overhaul every year. Long-term use experience shows that traditional hot-mix asphalt mixtures are greatly affected by heavy-load traffic, lack high temperature stability and water stability, and are prone to rutting, cracks, potholes and other diseases. In order to promote the green and low-carbon development of highway construction and maintenance technology, the application of waste polymers in the research of modified asphalt mixtures is a very promising and meaningful modification method. This technology involves two important aspects: one is the recycling of hazardous solid waste; the other is the improvement of the performance of pavement materials. In the engineering application of preparing modified asphalt mixtures using waste polymers, a variety of materials have been used as asphalt modifiers and have achieved good application results. The more well-known ones are waste tire rubber and waste engine oil. The results of engineering applications have proved that waste polymer modified asphalt mixture has significantly improved high temperature stability, water stability and other aspects compared with base asphalt mixture, while reducing the project cost and taking into account both high efficiency and economy.
[0003] In the prior art, asphalt mixture has the following problems:
[0004] 1. Asphalt mixture is a typical porous medium material, with a large number of tiny pores and cracks on the surface and internal structure. When water accumulates on the road or water penetrates into the internal pores and cannot be discharged in time, the adhesion between asphalt and aggregate decreases under the long-term effect of water environment, eventually leading to the peeling of asphalt film and the formation of cracks and pits (see Figure 1 ).
[0005] 2. Asphalt is a thermoplastic material. In southern my country, the highest temperature in summer can reach 40°C, and the road surface temperature exceeds 60°C. The asphalt mixture is in a mainly viscoelastic state, which causes its shear strength to be greatly reduced. At this time, the asphalt mixture is prone to plastic deformation under the action of vehicle load cycles, which gradually accumulates to form road rutting.
[0006] At present, modified asphalt is mainly modified by polymer modifiers, which are mainly divided into thermoplastic rubber, rubber and thermoplastic resin. These three types of modifiers are usually used to improve fatigue cracking resistance. Among them, thermoplastic rubber styrene butadiene styrene block copolymer (SBS) modified asphalt is the most widely used. SBS modified asphalt can effectively improve the high temperature stability and water stability of asphalt mixture, but SBS modified asphalt is difficult to process and has high cost. In addition, due to its high viscosity, the required production and construction temperatures are relatively high, resulting in relatively serious pollution emissions and energy consumption. Summary of the invention
[0007] The purpose of the present invention is to address the above-mentioned problems in the existing technology and propose a method for improving the performance of asphalt mixture by using waste circuit boards, which has the characteristics of improving the water damage resistance of the mixture and improving high temperature stability.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] A method for improving the performance of asphalt mixture by using waste circuit boards comprises the following steps:
[0010] S1. Crushing the circuit board and sieving out the original powder with a particle size of less than 0.075 mm;
[0011] S2, dropping a silane coupling agent into a 70% by mass ethanol solution to prepare a 2% by mass silane coupling agent solution;
[0012] S3, adding the original powder into a silane coupling agent solution for immersion treatment to obtain a modified powder;
[0013] S4. Mixing the modified powder with base asphalt to prepare modified asphalt, and finally mixing with aggregate to obtain a modified asphalt mixture, wherein the modified powder accounts for 8-14% by weight of the modified asphalt mixture.
[0014] In the above method for improving the performance of asphalt mixture by using waste circuit boards, in step S1, the circuit boards are waste circuit boards after metal components are recovered.
[0015] In the above method of improving the performance of asphalt mixture by using waste circuit boards, in step S1, at room temperature, water and anhydrous ethanol are used to prepare a 70% ethanol solution by mass, and a silane coupling agent is added dropwise to prepare a 2% silane coupling agent solution by mass.
[0016] In the above method of improving the performance of asphalt mixture by using waste circuit boards, in step S1, the circuit board scraps are crushed into 4.5-5.5 mm particles by a jaw crusher, then put into a high-speed pulverizer for secondary crushing, and finally sieved to obtain powder below 0.075 mm.
[0017] In the above method for improving the performance of asphalt mixture by using waste circuit boards, in step S3, the original powder is added to a silane coupling agent solution that has been hydrolyzed for at least 1 hour and immersed in it.
[0018] In the above method for improving the performance of asphalt mixture by using waste circuit boards, in step S3, the powder is dried after the soaking treatment and the powder is evenly dispersed.
[0019] In the above method for improving the performance of asphalt mixture by using waste circuit boards, in step S3, the weight difference between the modified powder after drying and the original powder before immersion treatment is less than 0.1% after weighing.
[0020] In the above method for improving the performance of asphalt mixture by using waste circuit boards, in step S3, the soaking time is 45-60 minutes.
[0021] Compared with the prior art, this application has the following advantages:
[0022] This technology uses non-metallic components of waste circuit boards as admixtures for the first time to improve the high temperature stability and water damage resistance of asphalt mixtures. According to the technical characteristics of hot mix asphalt mixtures, the crushing process, surface treatment process, admixture method and admixture amount of non-metallic components of waste circuit boards are proposed; the strength formation mechanism of asphalt mixtures modified by non-metallic components of waste circuit boards is explained. Under the optimal admixture amount and admixture method, the water damage resistance of the mixture can be improved by about 15%, and the high temperature stability can be improved by 40% to 50%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a diagram of the mechanism of action of water damage to asphalt mixture in this application;
[0024] Figure 2 It is a flow chart of the performance process of NMP modified asphalt mixture in this application;
[0025] Figure 3 It is a dissociation state diagram of NMP with different particle sizes in this application;
[0026] Figure 4 It is a microscopic morphology of the surface of non-metallic components of waste circuit boards before and after immersion in a silane coupling agent in this application;
[0027] Figure 5 It is the freeze-thaw splitting residual strength ratio diagram of the mixture under different NMP treatment methods. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Domestic research on the recycling and treatment technology of waste circuit boards started late. Due to the recycling value, there are endless technical studies on the recycling of precious metals in electronic waste, but very few studies on the recycling of non-metallic components. However, with the rapid development of materials science and environmental science, it is very conducive to the research and development of non-metallic components of waste circuit boards.
[0030] The main components of the non-metallic part (NMP) of waste circuit boards are cured epoxy resin and glass fiber. Resin materials have a certain improvement effect on the performance of asphalt, while glass fiber can play a reinforcing role. Both can be used as asphalt modifiers alone. Therefore, it is theoretically feasible to use the product obtained after processing the non-metallic components of waste circuit boards as an asphalt modifier. In addition, coarsely crushed circuit board fragments can also be used as fillers for asphalt mixtures. At present, most of the treatment solutions for the non-metallic parts of waste circuit boards are landfill and incineration, which not only wastes manpower and material resources, but also more seriously causes non-renewable damage to the atmosphere and soil. Using it as an asphalt modifier provides a new idea and new way of resource treatment, which can not only reduce the cost of modified asphalt, but also harmlessly treat harmful solid wastes, killing two birds with one stone, and has far-reaching economic, social and environmental significance. However, the application of waste circuit boards in asphalt mixtures has not yet been carried out at home and abroad.
[0031] Since waste circuit boards are in plate form when they are recycled, they cannot be directly modified in asphalt. They need to be crushed to meet the required fineness before they can be used as modifiers. At the same time, because the main components of the non-metallic part are epoxy resin and glass fiber, although they can be used as good fine-particle fillers and reinforcing fibers, the surface pH of the two components is mainly neutral, and there are problems with adhesion to asphalt. Therefore, it is of great significance to explore a production process for non-metallic component modifiers of waste circuit boards, which can be used as admixtures to improve the performance of asphalt mixtures.
[0032] The above problems all occur during the use and construction of asphalt mixtures. During road construction, it is necessary to consider the operability and economy of the construction process. Therefore, in view of the insufficient water stability and high temperature stability of asphalt mixtures, the characteristics of hot mix asphalt mixture mixing technology are comprehensively considered, and a construction process using non-metallic components of waste circuit boards to improve the high temperature stability and water damage resistance of asphalt mixtures is designed (see Figure 2 ).
[0033] A method for improving the performance of asphalt mixture by using waste circuit boards comprises the following steps:
[0034] S1. Crushing the circuit board and sieving out the original powder with a particle size of less than 0.075 mm;
[0035] In step S1, the circuit board adopts a non-metallic circuit board. The circuit board scraps are initially crushed into 4.5-5.5mm particles by a jaw crusher, and then put into a high-speed universal grinder for secondary crushing. Finally, powders below 0.075mm can be obtained by screening. After secondary crushing, the content of particles with a diameter of 0.075-0.15mm is the largest, accounting for about one-half; the content of particles below 0.075mm accounts for about one-third. In the powder with a particle size of 0.075-0.15mm, the glass fiber mainly exists in the form of long rods. Due to the cohesive effect of the resin matrix, most of the long rod-shaped glass fibers are covered with cured epoxy resin. On the other hand, the powder with a particle size of less than 0.075mm is dissociated more thoroughly during crushing, and there is much less resin attached to the surface of the glass fiber (see Figure 3 ). Powders below 0.075 mm can better play a reinforcing and filling role, so the particle size below 0.075 mm is selected as the target particle size of the modifier.
[0036] S2, dropping a silane coupling agent into a 70% by mass ethanol solution to prepare a 2% by mass silane coupling agent solution;
[0037] At room temperature, water and anhydrous ethanol are used to prepare an ethanol solution with a mass fraction of 70%, and a silane coupling agent is dropped into it to prepare a silane coupling agent solution with a mass fraction of 2%.
[0038] S3, adding the original powder into a silane coupling agent solution for immersion treatment to obtain a modified powder;
[0039] The original powder is added to the silane coupling agent solution after hydrolysis for at least 1 hour for soaking treatment, and further in step S3, the soaking time is 45-60 minutes. After the soaking treatment, the powder is dried and the powder is evenly dispersed. The modified powder after drying has a weight difference of less than 0.1% compared with the original powder before the soaking treatment after weighing.
[0040] The connection between silane coupling agent and inorganic materials relies on the chemical reaction between hydrolyzed silanol and inorganic hydroxyl groups, while the connection with organic materials is through the cross-linking and entanglement of the organic group -NH2 at the end of the molecule with the asphalt molecule, thus generating a strong physical entanglement and adsorption effect, which increases the viscosity of the asphalt (see Figure 4 ).
[0041] S4. Mixing the modified powder with base asphalt to prepare modified asphalt, and finally mixing with aggregate to obtain a modified asphalt mixture, wherein the modified powder accounts for 8-14% by weight of the modified asphalt mixture.
[0042] Based on the analysis of the strength formation mechanism of asphalt mixture and the characteristics of NMP, NMP was used as a modifier for the first time to improve the high temperature stability and water damage resistance of asphalt mixture. At the same time, according to the technical characteristics of hot mix asphalt mixture, the influence of NMP crushing process, surface treatment process, adding method and dosage on the performance of NMP modified asphalt mixture was explored and summarized. The mechanism of action of NMP on the mixture is as follows: NMP fully wraps with loose fine aggregate and asphalt to form a dense spatial network structure to interlock and reinforce the asphalt mortar and fill the larger gaps in the asphalt mixture. These three methods improve the performance of the mixture; NMP crushing process: first, the circuit board scraps are crushed into particles of about 5 mm by a jaw crusher, and then put into a high-speed universal crusher for secondary crushing, and finally sieved to obtain powder below 0.075 mm; the surface treatment method of NMP adopts the immersion method, and the rated mass of NMP is added to the silane coupling agent solution after hydrolysis for 1 hour and immersed for about 1 hour; the NMP adding process is: crushing NMP, then immersing NMP with silane coupling agent, and finally adding it directly into the mixing pot together with mineral material and asphalt; under the optimal dosage and addition method, the water damage resistance of the mixture can be improved by about 15%, and the high temperature stability can be improved by 40% to 50%.
[0043] The asphalt mixture will then be transported directly to the corresponding road surface, spread and compacted, and traffic will be allowed after the asphalt mixture cools down to room temperature.
[0044] The water stability and high temperature stability of asphalt mixtures are improved by adding modifiers. NMP can play a filling and reinforcing role in the mixture, which can effectively make up for the defects of asphalt such as insufficient high temperature stability. Its epoxy resin can also improve the anti-cracking performance of asphalt mortar. The principle of NMP improving the performance of the mixture is as follows: first, during the mixing process of the mixture, NMP can wrap loose fine aggregates with asphalt; secondly, NMP can fill the larger voids in the asphalt mixture, reduce the number of voids, and increase the density of the structure; and an appropriate amount of glass fiber can form a network structure in the asphalt mortar, which has an interlocking and reinforcing effect on the asphalt particles and mortar, and improves the density and stability of the asphalt mortar. Therefore, NMP is an ideal modifier for improving the road performance of asphalt mixtures.
[0045] On the basis of taking into account the performance improvement effect and economy of NMP on asphalt binder, the water stability (by molding standard Marshall specimens of asphalt mixture, testing the void ratio of the specimens and conducting splitting tests, and using the freeze-thaw splitting strength ratio to characterize the mixture's resistance to water damage) and high temperature stability (by molding and curing rutting specimens, and conducting 60°C rutting tests, using dynamic stability to characterize the mixture's high temperature stability) of asphalt mixtures at four NMP dosages of 8%, 10%, 12% and 14% were determined.
[0046] The NMP mentioned in this application is a non-metallic circuit board.
[0047] NMP is an ideal modifier for improving the road performance of asphalt mixture. By comparing two different ways of adding NMP: Method ①: only crushing NMP, and then adding it directly into the mixing pot together with mineral material and asphalt; Method ②: crushing NMP, and then soaking NMP with silane coupling agent, and finally adding it directly into the mixing pot together with mineral material and asphalt. The optimal addition process is obtained as Method ② (see Figure 5 and Table 1).
[0048] Table 1: Dynamic stability of mixtures under different NMP treatment methods
[0049]
[0050] The KH550 modified NMP asphalt mixture in Table 1 has a 10% dosage.
[0051] It should be noted that all directional indications in the embodiments of the present invention, such as up, down, left, right, front, back, etc., are only used to explain the relative position relationship and movement status of the components in a certain specific posture, as shown in the accompanying drawings. If the specific posture changes, the directional indication will also change accordingly.
[0052] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. At the same time, the meaning of "and / or" appearing in the full text is that it includes three schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0053] The above components are all common standard parts or components known to those skilled in the art, and their structures and principles can be known to those skilled in the art through technical manuals or conventional experimental methods.
[0054] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A method for improving the performance of asphalt mixture by using waste circuit boards. It is characterized in that The following steps are involved: S1. Crushing the circuit board and sieving out the original powder with a particle size of less than 0.075 mm; S2, dropping a silane coupling agent into a 70% by mass ethanol solution to prepare a 2% by mass silane coupling agent solution; S3, adding the original powder into a silane coupling agent solution for immersion treatment to obtain a modified powder; S4. Mixing the modified powder with base asphalt to prepare modified asphalt, and finally mixing with aggregate to obtain a modified asphalt mixture, wherein the modified powder accounts for 8-14% by weight of the modified asphalt mixture.
2. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 1, It is characterized in that In step S1, the circuit board is a waste circuit board from which metal components have been recovered.
3. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 1, It is characterized in that In step S1, at room temperature, water and anhydrous ethanol are used to prepare an ethanol solution with a mass fraction of 70%, and a silane coupling agent is dropped into it to prepare a silane coupling agent solution with a mass fraction of 2%.
4. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 1, It is characterized in that In step S1, the circuit board scraps are crushed into 4.5-5.5 mm particles by a jaw crusher, then put into a high-speed pulverizer for secondary crushing, and finally sieved to obtain powders below 0.075 mm.
5. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 1, It is characterized in that In step S3, the original powder is added to a silane coupling agent solution that has been hydrolyzed for at least 1 hour for immersion treatment.
6. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 5, It is characterized in that In step S3, the powder is dried after the soaking process and the powder is evenly dispersed.
7. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 1, It is characterized in that In step S3, the modified powder after drying has a weight difference of less than 0.1% compared with the original powder before the soaking treatment after weighing.
8. The method for improving the performance of asphalt mixture by using waste circuit boards according to claim 5, It is characterized in that In step S3, the soaking time is 45-60 minutes.