Environment-friendly solid waste recycled concrete and preparation method thereof
By optimizing the proportion of raw materials and adding high-efficiency water reducing agents, combined with gas induction agents and appropriate curing conditions, the problem of insufficient initial settling time and strength of environmentally friendly solid waste recycled concrete has been solved, performance improvement and resource recycling have been achieved, and the Sustainable development.
Patent Information
- Application Number
- CN202411152176.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The initial set time of environmentally friendly solid waste recycled concrete is long and the strength is low for 28 days, which leads to insufficient performance during use.
By optimizing the proportion of raw materials, adding high-efficiency water reducing agent, and accurately metering and even mixing during the preparation process, combining appropriate amount of gas induction agent and appropriate curing conditions, the strength and durability of concrete are improved, ensuring that it reaches its ideal within 28 days performance requirements.
It has achieved efficient initial condensation and strength improvement of concrete, maximized the use of solid waste in thermal power plants, reduced environmental pollution and maintenance frequency, and promoted resource recycling and sustainable development.
Smart Images

Figure CN118930153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to environmentally friendly solid waste recycled concrete and a preparation method thereof. Background Art
[0002] Environmentally friendly solid waste recycled concrete mainly refers to a new type of building material made by utilizing solid waste from thermal power plants and mixing it with raw materials such as cement and water in a certain proportion. The performance of this concrete is close to or reaches the standards of traditional concrete. At the same time, it can maximize the use of solid waste from thermal power plants (fly ash, desulfurization gypsum, slag), reduce and lower the damage to the natural environment and land occupation caused by the accumulation of solid waste from thermal power plants in ash dams.
[0003] However, since the environmentally friendly solid waste recycled concrete has a long initial setting time and low strength at 28 days, staff need to improve it. Summary of the invention
[0004] The object of the present invention is to provide an environmentally friendly solid waste recycled concrete and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] Environmentally friendly solid waste recycled concrete, including the following preparation raw materials:
[0007] 200-500 parts of fly ash, 200-500 parts of desulfurized gypsum, 30-200 parts of finished cement, 50-150 parts of slag, 150-250 parts of water and 1-10 parts of high-efficiency water reducing agent.
[0008] Preferably, the particle size of the fly ash is greater than or equal to 25 um, and the particle size of the slag is less than or equal to 25 mm.
[0009] The method for preparing environmentally friendly solid waste recycled concrete comprises the following steps:
[0010] S1. Raw material preparation;
[0011] S2, dry mixing;
[0012] S3, wet mixing molding;
[0013] S4. Pouring and curing.
[0014] Preferably, in step S1, the raw materials include fly ash, desulfurized gypsum, slag, finished cement, water and an appropriate amount of high-efficiency water reducing agent.
[0015] Preferably, in step S2, fly ash, desulfurized gypsum, slag, finished cement and high-efficiency water reducing agent are mixed evenly in a dry mixer in a predetermined proportion to form a dry-mixed mixture.
[0016] Preferably, in step S3, water and the dry mix are added to a wet mixer for wet mixing until a uniform concrete mixture is formed.
[0017] Preferably, in step S4, the concrete mixture is poured into the construction site or mold, vibrated and leveled, and then cured under suitable environmental conditions until the predetermined strength and performance requirements are reached.
[0018] Preferably, in step S1, the purity of the desulfurized gypsum is not less than 80%, and the high-efficiency water reducing agent can reduce the water-cement ratio of the concrete and improve the strength of the concrete.
[0019] Preferably, in step S3, by adjusting the stirring speed and stirring time to ensure that all raw materials are fully mixed, while controlling the slump and air content of the concrete, an appropriate amount of air entraining agent is added to the wet mix to improve the freeze-thaw resistance and durability of the concrete.
[0020] Preferably, in step S4, the curing process includes one or more of natural curing, steam curing and hot water curing, and the specific curing conditions are adjusted according to the ambient temperature, humidity and concrete mix ratio.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention reduces the water-cement ratio of concrete by adding a high-efficiency water reducing agent, thereby improving the strength of concrete. Secondly, without using recycled aggregate and mineral powder, by accurately measuring and reasonably adjusting the proportions of various raw materials, it is ensured that the concrete can achieve an ideal initial setting time (including final setting time) and effective concrete strength during use, thereby maximizing the use of solid waste (fly ash, desulfurized gypsum, slag) from thermal power plants, making "environmentally friendly solid waste recycled concrete" truly worthy of the name, promoting the recycling of resources, and being conducive to sustainable development.
[0023] (2) No toxic or harmful substances are produced during the preparation process, which reduces pollution to the environment. The finished concrete has good durability and resistance to environmental erosion, which helps reduce the frequency of maintenance and reconstruction of buildings during use, further reducing the impact on the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a preparation flow chart of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] See also Figure 1 As shown, the environmentally friendly solid waste recycled concrete includes the following preparation raw materials:
[0028] 200-500 parts of fly ash, 200-500 parts of desulfurized gypsum, 30-200 parts of finished cement, 50-150 parts of slag, 150-250 parts of water and 1-10 parts of high-efficiency water reducing agent.
[0029] The particle size of fly ash is greater than or equal to 25um, and the particle size of slag is less than or equal to 25mm.
[0030] The method for preparing environmentally friendly solid waste recycled concrete comprises the following steps:
[0031] S1. Raw material preparation;
[0032] S2, dry mixing;
[0033] S3, wet mixing molding;
[0034] S4. Pouring and curing.
[0035] In step S1, the raw materials include fly ash, desulfurized gypsum, slag, finished cement, water and an appropriate amount of high-efficiency water reducing agent.
[0036] Fly ash treatment: Select high-quality fly ash and ensure that its key indicators such as fineness and water demand ratio meet the standards to reduce the adverse effects on concrete performance. Fly ash needs to be dried before use to remove excess moisture and improve mixing efficiency.
[0037] Desulfurized gypsum quality control: As an important mineral admixture, the purity of desulfurized gypsum directly affects the performance of concrete. Ensure that the purity is not less than 80%, and test its chemical composition to avoid harmful impurities.
[0038] High-efficiency water reducing agent: Polycarboxylic acid-based high-efficiency water reducing agent is selected because of its excellent water-reducing effect and good working performance. It can effectively reduce the water-cement ratio of concrete and improve strength and durability.
[0039] In step S2, fly ash, desulfurized gypsum, finished cement, mineral powder and high-efficiency water reducing agent are mixed evenly in a dry mixer according to a predetermined ratio to form a dry-mixed mixture.
[0040] Accurate measurement: Use electronic scales and other precision measuring equipment to ensure that the proportion of various raw materials is accurate.
[0041] Uniform mixing: In the dry mixer, fly ash, desulfurized gypsum, slag, finished cement and high-efficiency water reducer are fully and evenly mixed through strong stirring to form a dense dry-mixed mixture. In this process, the stirring time and stirring speed must be controlled to avoid excessive stirring that may cause material agglomeration.
[0042] In step S3, recycled aggregate and water are added to the dry-mixed mixture, and wet mixing is performed in a wet mixer until a uniform concrete mixture is formed. The mixing speed and mixing time are adjusted to ensure that all raw materials are fully mixed, and the slump and air content of the concrete are controlled. An appropriate amount of air entraining agent is added to the wet-mixed mixture to improve the freeze-thaw resistance and durability of the concrete.
[0043] Moisture control: Accurately calculate the required amount of water based on the concrete mix ratio and the state of raw materials to ensure that the concrete mixture has appropriate slump and workability.
[0044] Wet mixing process: Gradually add recycled aggregate and water to the dry mix, and fully stir in a wet mixer until a uniform, lump-free concrete mixture is formed. During this process, an appropriate amount of air-entraining agent can be added to introduce tiny bubbles to improve the freeze-thaw resistance and durability of the concrete.
[0045] Performance adjustment: By adjusting the mixing parameters and the amount of additives, the key performance indicators of concrete such as slump and air content can be controlled to meet the needs of different projects.
[0046] In step S4, the concrete mixture is poured into a mold, and after being vibrated and smoothed, it is cured under suitable environmental conditions until the predetermined strength and performance requirements are reached. The curing process includes one or more of natural curing, steam curing and hot water curing. The specific curing conditions are adjusted according to the ambient temperature, humidity and concrete mix ratio.
[0047] Mold preparation: Select a suitable mold to ensure accurate size and smooth surface to facilitate demoulding and subsequent processing.
[0048] Pouring and vibrating: Pour the concrete mixture evenly into the mold and vibrate it with a vibrating rod or vibrating table to remove bubbles and excess moisture and improve the density and strength of the concrete.
[0049] Maintenance management: Develop a scientific maintenance plan based on ambient temperature, humidity and concrete mix ratio. Natural maintenance, steam maintenance or hot water maintenance can be used to ensure that the concrete hardens and develops strength under suitable conditions. At the same time, strengthen monitoring and management during maintenance to promptly identify and handle possible problems.
[0050] Resource recycling: The large-scale use of industrial waste and recycled aggregates such as fly ash and desulfurized gypsum has effectively reduced the exploitation of natural resources and the discharge of construction waste, and promoted the recycling of resources.
[0051] Energy saving and emission reduction: By optimizing the mix ratio and adopting high-efficiency water-reducing agents and other measures, the water-cement ratio of concrete and the amount of cement per unit volume are reduced, thereby reducing energy consumption and carbon emissions.
[0052] Environmentally friendly: No toxic or harmful substances are produced during the preparation process. The finished concrete has good durability and resistance to environmental erosion, which helps to extend the service life of buildings and reduce the environmental impact caused by maintenance and reconstruction.
[0053] Embodiment 2:
[0054] See also Figure 1 As shown, the environmentally friendly solid waste recycled concrete includes the following preparation raw materials:
[0055] 300 parts of fly ash, 200 parts of desulfurized gypsum (purity 90%), 100 parts of slag, 180 parts of finished cement, 150 parts of water, and 5 parts of high-efficiency water reducing agent.
[0056] The method for preparing environmentally friendly solid waste recycled concrete comprises the following steps:
[0057] Raw material preparation: Ensure that all raw materials meet quality standards, especially recycled aggregates are strictly screened and processed to reduce impurities and micro cracks.
[0058] Dry mixing: In a dry mixer, fly ash, desulfurized gypsum, finished cement and high-efficiency water reducing agent are mixed evenly in the above proportions to form a dry mixture.
[0059] Wet mix: Add recycled aggregate and water to the dry mix and mix in a wet mixer for 5 minutes to form a uniform concrete mixture. During this period, 0.05% of air entraining agent is added to improve the freeze-thaw resistance of the concrete.
[0060] Pouring and curing: Pour the concrete mixture into a standard mold, vibrate and smooth it, and then steam cure it for 7 days at 20°C and 90% humidity, and then naturally cure it for 28 days.
[0061] Compressive strength: The compressive strength after 28 days reaches 16.2MPa.
[0062] Flexural strength: 28-day flexural strength is 4.7MPa.
[0063] Freeze-thaw cycle resistance: After 100 freeze-thaw cycles, the strength loss is less than 5%.
[0064] Slump: The initial slump is 180mm and 160mm after 1 hour.
[0065] High-efficiency water reducing agent: Polycarboxylic acid-based high-efficiency water reducing agent is selected because of its excellent water-reducing effect and good working performance. It can effectively reduce the water-cement ratio of concrete and improve strength and durability.
[0066] In step S2, fly ash, desulfurized gypsum, finished cement and high-efficiency water reducing agent are mixed evenly in a dry mixer according to a predetermined ratio to form a dry-mixed mixture.
[0067] Accurate measurement: Use electronic scales and other precision measuring equipment to ensure that the proportion of various raw materials is accurate.
[0068] Uniform mixing: In the dry mixer, fly ash, desulfurized gypsum, finished cement, mineral powder and high-efficiency water reducer are fully and evenly mixed through strong stirring to form a dense dry-mixed mixture. In this process, the stirring time and stirring speed must be controlled to avoid excessive stirring that may cause material agglomeration.
[0069] In step S3, recycled aggregate and water are added to the dry-mixed mixture, and wet mixing is performed in a wet mixer until a uniform concrete mixture is formed. The mixing speed and mixing time are adjusted to ensure that all raw materials are fully mixed, and the slump and air content of the concrete are controlled. An appropriate amount of air entraining agent is added to the wet-mixed mixture to improve the freeze-thaw resistance and durability of the concrete.
[0070] Moisture control: Accurately calculate the required amount of water based on the concrete mix ratio and the state of raw materials to ensure that the concrete mixture has appropriate slump and workability.
[0071] Wet mixing process: Gradually add recycled aggregate and water to the dry mix, and fully stir in a wet mixer until a uniform, lump-free concrete mixture is formed. During this process, an appropriate amount of air-entraining agent can be added to introduce tiny bubbles to improve the freeze-thaw resistance and durability of the concrete.
[0072] Performance adjustment: By adjusting the mixing parameters and the amount of additives, the key performance indicators of concrete such as slump and air content can be controlled to meet the needs of different projects.
[0073] In step S4, the concrete mixture is poured into a mold, and after being vibrated and smoothed, it is cured under suitable environmental conditions until the predetermined strength and performance requirements are reached. The curing process includes one or more of natural curing, steam curing and hot water curing. The specific curing conditions are adjusted according to the ambient temperature, humidity and concrete mix ratio.
[0074] Mold preparation: Select a suitable mold to ensure accurate size and smooth surface to facilitate demoulding and subsequent processing.
[0075] Pouring and vibrating: Pour the concrete mixture evenly into the mold and vibrate it with a vibrating rod or vibrating table to remove bubbles and excess moisture and improve the density and strength of the concrete.
[0076] Embodiment three:
[0077] See also Figure 1 As shown, the environmentally friendly solid waste recycled concrete includes the following preparation raw materials:
[0078] 250 parts of fly ash, 150 parts of desulfurized gypsum (purity 90%), 100 parts of slag, 150 parts of finished cement, 120 parts of water, and 10 parts of high-efficiency water reducing agent.
[0079] Raw material preparation: Recycled aggregates undergo special treatments, such as pre-treatment with surfactants, to reduce water absorption and improve bonding with cement.
[0080] Dry mixing: Use a high-efficiency dry mixer to evenly mix fly ash, desulfurized gypsum, finished cement and high-efficiency water reducing agent.
[0081] Wet mixing: During the wet mixing process, the mixing speed is controlled at 30 revolutions per minute and the mixing time is 6 minutes to ensure that the concrete mixture is uniform and free of lumps.
[0082] Casting and curing: Use hot water curing method, curing in 60℃ hot water for the first 3 days, and then switch to natural curing for 28 days.
[0083] Compressive strength: The compressive strength after 28 days reaches 22.6MPa.
[0084] Flexural strength: 28-day flexural strength is 6.5MPa.
[0085] Shrinkage: The shrinkage after 28 days is 0.03%, showing good volume stability.
[0086] Durability: After 6 months of exposure testing in a chloride ion corrosion environment, no obvious signs of corrosion were found on the concrete surface.
[0087] High-efficiency water reducing agent and mineral powder: Polycarboxylic acid-based high-efficiency water reducing agent is selected because of its excellent water-reducing effect and good working performance. It can effectively reduce the water-cement ratio of concrete and improve strength and durability.
[0088] In step S2, fly ash, desulfurized gypsum, finished cement and high-efficiency water reducing agent are mixed evenly in a dry mixer according to a predetermined ratio to form a dry-mixed mixture.
[0089] Accurate measurement: Use electronic scales and other precision measuring equipment to ensure that the proportion of various raw materials is accurate.
[0090] Uniform mixing: In the dry mixer, fly ash, desulfurized gypsum, finished cement, mineral powder and high-efficiency water reducer are fully and evenly mixed through strong stirring to form a dense dry-mixed mixture. In this process, the stirring time and stirring speed must be controlled to avoid excessive stirring that may cause material agglomeration.
[0091] In step S3, recycled aggregate and water are added to the dry-mixed mixture, and wet mixing is performed in a wet mixer until a uniform concrete mixture is formed. The mixing speed and mixing time are adjusted to ensure that all raw materials are fully mixed, and the slump and air content of the concrete are controlled. An appropriate amount of air entraining agent is added to the wet-mixed mixture to improve the freeze-thaw resistance and durability of the concrete.
[0092] Moisture control: Accurately calculate the required amount of water based on the concrete mix ratio and the state of raw materials to ensure that the concrete mixture has appropriate slump and workability.
[0093] Wet mixing process: Gradually add recycled aggregate and water to the dry mix, and fully stir in a wet mixer until a uniform, lump-free concrete mixture is formed. During this process, an appropriate amount of air-entraining agent can be added to introduce tiny bubbles to improve the freeze-thaw resistance and durability of the concrete.
[0094] Performance adjustment: By adjusting the mixing parameters and the amount of additives, the key performance indicators of concrete such as slump and air content can be controlled to meet the needs of different projects.
[0095] In step S4, the concrete mixture is poured into a mold, and after being vibrated and smoothed, it is cured under suitable environmental conditions until the predetermined strength and performance requirements are reached. The curing process includes one or more of natural curing, steam curing and hot water curing. The specific curing conditions are adjusted according to the ambient temperature, humidity and concrete mix ratio.
[0096] Mold preparation: Select a suitable mold to ensure accurate size and smooth surface to facilitate demoulding and subsequent processing.
[0097] Pouring and vibrating: Pour the concrete mixture evenly into the mold and vibrate it with a vibrating rod or vibrating table to remove bubbles and excess moisture and improve the density and strength of the concrete.
[0098] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0099] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0100] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0101] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0102] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Environmentally friendly solid waste recycled concrete, It is characterized in that The preparation includes the following raw materials: 200-500 parts of fly ash, 200-500 parts of desulfurized gypsum, 50-150 parts of slag, 30-200 parts of finished cement, 150-250 parts of water and 1-10 parts of high-efficiency water reducing agent.
2. The environmentally friendly solid waste recycled concrete according to claim 1, Features: The particle size of the fly ash is greater than or equal to 25um, and the particle size of the slag is less than or equal to 25mm.
3. A method for preparing environmentally friendly solid waste recycled concrete, applicable to the environmentally friendly solid waste recycled concrete according to claims 1 to 2, It is characterized in that The following steps are involved: S1. Raw material preparation; S2, dry mixing; S3, wet mixing molding; S4. Pouring and curing.
4. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S1, the raw materials include fly ash, desulfurized gypsum, slag, finished cement, water and an appropriate amount of high-efficiency water reducing agent.
5. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S2, fly ash, desulfurized gypsum, slag, finished cement and high-efficiency water reducing agent are mixed evenly in a dry mixer according to a predetermined ratio to form a dry-mixed mixture.
6. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S3, water and the dry mix are added into a wet mixer for wet mixing until a uniform concrete mixture is formed.
7. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S4, the concrete mixture is poured into the construction site or mold, vibrated and leveled, and then cured under suitable environmental conditions until the predetermined strength and performance requirements are reached.
8. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S1, the purity of the desulfurized gypsum is not less than 80%, and the high-efficiency water reducing agent can reduce the water-cement ratio of the concrete and improve the strength of the concrete.
9. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S3, the mixing speed and mixing time are adjusted to ensure that all raw materials are fully mixed, while the slump and air content of the concrete are controlled, and an appropriate amount of air entraining agent is added to the wet mix to improve the freeze-thaw resistance and durability of the concrete.
10. The method for preparing the environmentally friendly solid waste recycled concrete according to claim 3, Features: In step S4, the curing process includes one or more of natural curing, steam curing and hot water curing, and the specific curing conditions are adjusted according to the ambient temperature, humidity and concrete mix ratio.
Citation Information
Cited By
Calcined stone self-compacting concrete as well as preparation method and application thereof
CN119899018A