Roadbed filler for treating tunnel excavation waste salinized loess based on curing agent and preparation method of roadbed filler

By adding components such as magnesium slag and fly ash to tunnel waste, a stable phase such as ettringite is generated, which solves the problem of unstable strength of hydrated loess in tunnels during the hydration process, realizes high-strength and water-stable roadbed filler, and promotes the comprehensive utilization of tunnel waste.

CN118930159AActive Publication Date: 2024-11-12CHINA MCC17 GRP CO LTD

Patent Information

Application Number
CN202411208120.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively treat saline loess generated during tunnel excavation, resulting in unstable strength when exposed to water and a high content of sulfates, which fails to meet the technical requirements for roadbed fillers.

Method used

A roadbed filler based on curing agent treatment of saline loess waste from tunnel excavation is adopted, which includes a combination of tunnel waste, magnesium slag, fly ash, activator, reinforcing agent and adsorbent. By controlling the proportion of each component and the hydration reaction, stable phases such as ettringite and hydrated magnesium aluminosilicate gel are generated, thereby improving the strength and stability of the material.

Benefits of technology

The generated stable phase significantly improves the strength and water stability of the subgrade filler, meets the technical requirements of highway subgrade, reduces porosity, enhances the overall performance of the material, and is suitable for the comprehensive utilization of tunnel waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930159A_ABST
    Figure CN118930159A_ABST
Patent Text Reader

Abstract

The invention discloses a roadbed filler for treating tunnel excavation waste salinized loess based on a curing agent and a preparation method of the roadbed filler, and belongs to the technical field of comprehensive utilization of tunnel spoil, the roadbed filler comprises tunnel waste residues, the curing agent and water, the curing agent comprises 23-27 parts of magnesium slag, 3-5 parts of fly ash, 1-3 parts of an exciting agent, 6-8 parts of a reinforcing agent and 3-5 parts of an adsorbent, and the curing agent comprises a curing agent and a curing agent. The adsorbent is magnesium aluminum carbonate hydrotalcite. According to the method, high-content sulfate radicals in the tunnel waste residues are fully utilized, hydrated magnesium aluminosilicate and hydrated calcium aluminosilicate gel are generated by a curing agent in the curing process, and the hydrated magnesium aluminosilicate, the hydrated calcium aluminosilicate and cations in magnesium aluminum carbonate hydrotalcite are subjected to ion exchange and synergistic reaction to form a stable phase; the mechanical property and the environmental stability of the solidified soil are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of comprehensive utilization of tunnel waste soil, and more specifically, relates to a roadbed filler for treating salinized loess abandoned from tunnel excavation based on a curing agent and a preparation method thereof. Background Art

[0002] With the economic development of the western region, more and more highways are being built in the western mountainous areas. The biggest feature of mountainous highways is that the ratio of bridges and tunnels is very high, generally more than 50%. Some highways such as the Sichuan Guanggan Expressway have a ratio of bridges and tunnels as high as 80%. The number of long tunnels, extra-long tunnels and tunnel groups is increasing day by day, and the more tunnels are excavated, the more tunnel spoil is generated. Due to the limitations of construction technology, construction management conditions and other aspects, the utilization of tunnel spoil is not perfect, the utilization method is relatively single, and the tunnel spoil is not fully and comprehensively utilized as high-quality road construction materials. The utilization rate is generally low, only about 20%. Tunnel spoil requires a large amount of land, and also causes waste of resources and environmental pollution, and will form potential soil and water loss problems. Therefore, the comprehensive utilization of tunnel spoil in mountainous areas and the optimization of resource allocation and use are issues that need to be urgently solved in highway construction, especially in mountainous highway construction.

[0003] Fenghuangshan Tunnel is an important node project of the Qingshuiyi to Zhonghe section of the G30 Lianhuo Expressway. It is located in Jinya Town, Yuzhong County, Lanzhou City. It is designed as a long double-hole tunnel with left and right lanes separated. It is 3,945 meters long and is an extra-long tunnel with a maximum burial depth of 180 meters. During the excavation and construction process, a large amount of abandoned tunnel engineering loess was generated.

[0004] Patent CN116143468A discloses a premixed fluidized solidified saline soil and its preparation method. The premixed fluidized solidified saline soil is mainly made of clay soil containing chloride salts in coastal areas, and includes the following raw materials by mass: 80-100 parts of saline soil, 25-30 parts of iron tailings sand, 6-8 parts of cement, 8-10 parts of slag, 5-7 parts of steel slag, 3-4 parts of fly ash, 1.2-1.4 parts of magnesium salt, 0.7-0.9 parts of activator, 0.4-0.6 parts of water reducer, 65-70 parts of water, but the saline soil in the patent. The premixed fluidized solidified saline soil in the patent is mainly for clay soil containing chloride salts. Its curing agent formula contains a high proportion of iron tailings sand, slag and steel slag. These materials have good salt erosion resistance in a high chloride salt environment, and the initial strength of the soil body is improved through the synergistic effect of cement and activator. However, this formula is mainly for clay soil and chloride environment, and may not be suitable for sulfate environment in tunnel waste. The presence of sulfate may cause calcium ions in cement and slag to react with sulfate ions to generate expansive products (such as gypsum), thereby affecting the curing effect. Therefore, the curing agent of this patent may face the problem of generating expansive salts when treating tunnel waste, and cannot be used directly.

[0005] Patent CN117088626A discloses a fully solid waste soil stabilizer for stabilizing saline soil and a preparation method thereof. The fully solid waste soil stabilizer for stabilizing saline soil provided by the present invention comprises 20 to 50 parts of carbide slag, 10 to 40 parts of slag, 10 to 30 parts of furnace slag, 10 to 30 parts of recycled micro powder of brick-concrete construction waste and 5 to 15 parts of modified desulfurized gypsum; wherein CaO accounts for 35% to 50%, Al 2 O 3 and SiO 2 The total amount accounts for 30% to 45%, Fe 2 O 3 , MgO and SO 3 The total amount accounts for 5% to 20%, and other chemical components account for 2% to 10%. The saline soil in this patent The curing agent in this patent is designed to stabilize saline soil. It uses all solid waste materials, such as carbide slag, slag, slag and modified desulfurized gypsum, and is suitable for high-salinity soil. Its high CaO content can effectively increase the alkalinity of the soil and contribute to the formation of calcium sulfonite and other stable phases. However, this curing agent is mainly aimed at high salinity, especially environments containing sulfates and chlorides. Although its ingredients include carbide slag and slag, it has strong activity and reactivity, but in tunnel waste slag, due to the complex composition containing rock fragments and other impurities and the high salt concentration, the effect of this curing agent may be limited, especially when the ratio is not adjusted, which may lead to the formation of expansion products or insufficient curing effect. Summary of the invention

[0006] 1. Problem to be solved

[0007] In view of the problem that excessive sulfate ions in existing saline soil lead to unstable strength when exposed to water, the present invention provides a roadbed filler based on curing agent treatment of abandoned salinized loess from tunnel excavation and a preparation method thereof. The prepared roadbed filler has certain strength and water stability, and meets the technical requirements for filling highway roadbeds.

[0008] 2. Technical solution

[0009] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0010] A roadbed filler for treating salinized loess abandoned from tunnel excavation based on a curing agent. The roadbed filler comprises tunnel waste, a curing agent and water. The dry mass ratio of the tunnel waste to the curing agent is 1:0.08-0.12, and the moisture content of the tunnel waste is controlled at 15%-16%.

[0011] Among them, the amount of curing agent added and the water content affect the formation of hydration products.

[0012] The curing agent includes magnesium slag, fly ash, an activator, a reinforcing agent and an adsorbent:

[0013] The weight proportions of the components are as follows: 23-29 parts of magnesium slag, 3-9 parts of fly ash, 1-3 parts of activator, 6-8 parts of enhancer and 3-5 parts of adsorbent.

[0014] Preferably, the apparent density of the magnesium slag is 3000-3250 kg / m 3 The particle size is 2 to 4 mm. If its content is too much, it may increase the alkalinity, causing the material to crack or expand during the later curing process, affecting the overall stability; if its content is too little, the amount of gelling products such as hydrated magnesium aluminosilicate in the material will be reduced, resulting in a decrease in the strength and compressive resistance of the material.

[0015] Preferably, the activator is a mixture of carbide slag and desulfurized gypsum, with a mass ratio of 9 to 10:1. Excessive content may lead to an intensified alkali-silicon reaction of the material, resulting in microcracks, and reducing the durability and crack resistance of the material. In addition, excessive activator may cause the volume stability of the material to deteriorate and expand; too little content will lead to a reduction in the production of gelling products such as hydrated calcium silicate and hydrated calcium aluminosilicate. This will directly affect the strength, density and durability of the material, and it will not meet the mechanical and durability requirements in engineering applications.

[0016] Preferably, the reinforcing agent is steel slag powder with a particle size of ≤200 μm. Too much steel slag powder may increase the rigidity of the material, making the material more brittle when subjected to external force, resulting in reduced impact resistance. At the same time, too much steel slag powder may increase the density of the material, making its construction operability worse and possibly increasing the cost of the material; too little steel slag powder may make the microstructure of the material less dense, affecting the overall stability of the material.

[0017] Preferably, the adsorbent is magnesium carbonate aluminum hydrotalcite, which needs to be baked in a muffle furnace at 490-510°C for 3 hours in advance. Too much of it may affect the curing speed of the material, resulting in extended curing time during construction; too little of it may cause the excess harmful ions (such as sulfates) in the material to fail to be effectively adsorbed and fixed, so that the material may swell or lose strength during long-term use, affecting its durability and stability.

[0018] The carbonate ions inside magnesium aluminum carbonate hydrotalcite affect its adsorption effect. In order to enhance the adsorption effect of magnesium aluminum carbonate hydrotalcite, it is necessary to replace the carbonate ions inside magnesium aluminum carbonate hydrotalcite in advance so that they can more effectively exchange with the target ions or molecules in the subsequent adsorption process.

[0019] If too much curing agent is added, there will be an excess of reactants in the material, which may result in incompletely reacted curing agent remaining in the material. This will not only increase the cost of the material, but may also cause local excessive alkalinity inside the material, thereby increasing the risk of cracking or swelling of the material. If too little curing agent is added, the hydration reaction will be incomplete, the amount of gelled product generated will be reduced, and the strength and durability of the material will be insufficient. In addition, insufficient curing agent may not be able to fully neutralize harmful ions or particles in the material, which will greatly reduce the durability and stability of the material and fail to meet engineering requirements.

[0020] If the water content is too high, the hydration reaction rate in the material may be accelerated, but it may also cause too many pores to form inside the material, thereby reducing its density and compressive strength. In addition, excessive water content may also make the curing reaction uneven, resulting in unstable material properties. If the water content is too low, the hydration reaction will be restricted, and the generated gel products will be reduced, resulting in a significant decrease in the strength and durability of the material. It may also make it difficult to fully compact the material during the molding process, forming an uneven microstructure and affecting the overall stability of the material. In addition, insufficient water may cause the active components in the curing agent to be unable to fully dissolve and diffuse, affecting the reaction and the formation of hydration products.

[0021] Preferably, 95-98% of the tunnel waste is loess, and 2-5% is rock debris. According to the liquid limit and plastic limit combined determination test, the liquid limit is 29.2%, and the plastic limit index is 10.9, which belongs to low plastic clay.

[0022] Preferably, among the tunnel waste slag, 19% to 20% has a particle size of less than 0.005 mm, 77% to 78% has a particle size of 0.005 mm to 0.075 mm, and 2% to 3% has a particle size of 0.075 mm to 2 mm.

[0023] Preferably, the total amount of soluble salt in the tunnel waste is 3.0% to 3.1%, the total amount of chloride ions is 0.20% to 0.30%, and the concentration of sulfate ions is 1.10% to 1.30%, which belongs to strong sulfate soil. 4 2- / Cl - >2.

[0024] The present invention also provides a method for preparing the roadbed filler based on curing agent treatment of abandoned salinized loess from tunnel excavation, comprising the following steps:

[0025] The tunnel waste soil, curing agent and water are mixed and then molded and cured in sequence to obtain the roadbed filling material.

[0026] Preferably, the curing is constant temperature and humidity curing; the curing temperature is 23±1°C, the relative humidity is 98%, and the curing age is set to 7 days, 14 days, or 28 days.

[0027] Preferably, the specimens with a curing age of 28 days are immersed in distilled pure water on the 27th day and the curing is continued for 24 hours; the vertical distance between the water surface and the top of the specimen is 2.5 cm.

[0028] Preferably, the forming method is static compaction.

[0029] The 7d unconfined compressive strength of the obtained roadbed filler is greater than 1.70MPa; the 28d unconfined compressive strength is greater than 7.84MPa; the water stability coefficient is 70-80%, and the present invention overcomes the problem of water instability in the original scheme; at the same time, the sulfate ion concentration is also significantly reduced, and the leaching concentration reaches the national groundwater quality Class IV standard.

[0030] This application is aimed at the comprehensive utilization of abandoned salinized loess. This type of abandoned loess is not only unstable in strength when exposed to water, but also contains a large amount of sulfate, and has some engineering properties of saline soil, such as high salt content, poor soil structure, low soil fertility, and soil moisture conditions are affected by salt concentration. Therefore, during on-site construction, the construction team generally uses 5% slaked lime curing agent to mix into the abandoned salinized loess, and cooperates with geomembranes, geotextiles and other physical reinforcement methods to reduce the adverse effects of engineering abandoned salinized loess. However, this type of treatment method still has many defects that need to be improved, such as poor water stability, high cost, environmental pollution, low strength, and excessive sulfate ions.

[0031] It should be noted that the present invention is mainly aimed at engineering waste residues with excessive sulfate content, rather than engineering waste residues with excessive chloride content. When chloride reacts with materials such as cement and lime, the products generated are relatively simple, mainly compounds such as calcium chloride. Therefore, the solidification of chloride engineering waste residues mainly relies on physical effects rather than complex chemical reactions, such as patent CN117088626A. However, in the present invention, for engineering waste residues with excessive sulfate content (such as calcium sulfate and sodium sulfate), the opposite is done, and the "harmful" component Cl therein is utilized. - and SO 4 2- Through chemical reactions, hydration products that are beneficial to the mechanical properties of the solidified soil are generated, such as AFt (ettringite), Friedel salt and Kuzel salt, forming a dense solidified body, thereby significantly improving the strength and stability of the soil.

[0032] 3. Beneficial effects

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The roadbed filler of the present invention makes full use of the high content of sulfate in the tunnel waste slag. During the solidification process of the tunnel waste slag, the calcium carbide slag in the curing agent and the tunnel waste slag generate hydrated magnesium aluminosilicate and hydrated calcium aluminosilicate gels. The hydrated magnesium aluminosilicate and hydrated calcium aluminosilicate undergo ion exchange and synergistic reaction with the cations in the magnesium aluminum carbonate hydrotalcite to form a stable phase, thereby effectively improving the mechanical properties and environmental stability of the solidified soil.

[0035] (2) The tunnel waste slag of the roadbed filler of the present invention contains rock fragments. After the pyrite rock fragments are mixed with carbide slag, the FeS 2 The hydrolysis of ions produces more sulfate ions, which in turn produces more calcium vanadate and Friedel salt. At the same time, the SiO 2 The glass structure is decomposed to generate more CAH and CASH structures. These hydration products are gelled together, which significantly improves the strength of the solidified soil, reduces the porosity, and improves the strength of the roadbed filler.

[0036] (3) The roadbed filler of the present invention improves the strong alkalinity of tunnel waste slag by adding carbide slag, increases the pH value of the soil solution, destroys the binding of soil particles to sulfate ions, thereby enhancing the accessibility of sulfate ions and improving the adsorption capacity of magnesium aluminum carbonate hydrotalcite to sulfate ions in the soil;

[0037] (4) The present invention uses tunnel waste slag with a smaller particle size distribution as the matrix material. The material with a smaller particle size has a larger specific surface area, which helps to accelerate the hydration reaction and uniformly generate hydration products, reduce porosity, and enhance the overall strength and stability of the material. In a high alkalinity environment, it is easier to form uniform CASH and MASH gels, further promoting the generation of stable phases such as ettringite and layered double hydroxides. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.

[0039] Figure 1 is the particle gradation curve of the tunnel waste soil of the present invention;

[0040] Figure 2 This is a microstructure photograph of the hydration product of the present invention. DETAILED DESCRIPTION

[0041] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments of the present invention that can be implemented are shown as examples. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is only for the purpose of illustrating and not limiting the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.

[0042] It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention. As used herein, the terms "parallel" and "perpendicular" are not limited to their strict geometric definitions, but include tolerances for reasonable and inconsistent machining or human errors.

[0043] By using local industrial solid waste in Gansu Province as admixtures, the comprehensive utilization rate of tunnel slag is improved. It not only realizes large-scale, low-cost, high-value-added solid waste resource utilization, but also avoids the long-distance transportation of slag, turning tunnel slag into treasure, greatly reducing the construction cost and comprehensive carbon emissions in roadbed projects in Gansu, and has high economic and environmental benefits.

[0044] The tunnel waste slag used in the present invention is taken from the excavation waste soil of Fenghuangshan Tunnel in the Lanzhou section of G30 Lianyungang to Horgos Expressway in Lanzhou City, Gansu Province. The soil is yellow-brown, blocky, and has cracks. After drying and crushing, its particle size and gradation are as follows: 20.96% of tunnel waste slag with a particle size of less than 0.005mm, 77.48% of tunnel waste slag with a particle size of 0.005mm to 0.075mm, and 1.56% of tunnel waste slag with a particle size of 0.075mm to 2mm. The selected curing agents include fly ash and magnesium slag, both of which are purchased from Nanjing City, Jiangsu Province. The particle size distribution is as follows: Figure 1 The main chemical components and their contents are shown in Table 1.

[0045] Table 1 Chemical composition and content of each solid waste

[0046] Material <![CDATA[Al 2 THE 3 ]]> <![CDATA[SiO 2 ]]> CaO <![CDATA[Fe 2 THE 3 ]]> MgO <![CDATA[SO 3 ]]> Tunnel waste 16.27 58.49 9.36 5.10 3.89 0.75 Fly ash 37.25 44.65 6.91 4.59 1.68 1.28 Magnesium slag 1.31 30.73 45.09 10.08 11.26 0.12

[0047] The preparation process of the roadbed filler of the embodiment and comparative example comprises the following steps:

[0048] A. Wetting of waste soil:

[0049] First, put the soil into an oven and dry it at 105℃. Then, crush it with a wooden hammer and a wooden roller and pass it through a 5mm sieve. Spread the sieve on a square plate and spray the required amount of water evenly with a sprayer to reach the target moisture content. Mix it again. Then put the wetted waste soil into a woven bag lined with polyvinyl chloride and seal it for at least 24 hours to evenly distribute the pore water of the waste soil. Collect wetted soil samples at a sampling frequency of 1 soil sample per kilogram to test the moisture content, ensuring that the maximum difference in moisture content is within 1%.

[0050] B. Mixing of curing agent and waste soil:

[0051] The weighed curing agent was added to the wetted waste soil prepared in step A and mixed until the mixture had no obvious color difference. The mixture was then stirred for 5 minutes using an NJ-160 tabletop cement paste electric mixer to further increase its uniformity. After stirring, the uniformly mixed solidified soil sample was transferred to a polyethylene plastic basin and covered with plastic wrap to prevent water evaporation. In order to avoid cross contamination between solidified soil samples, the stirring pot and stirring blades were thoroughly cleaned after the preparation of different solidified soil samples.

[0052] C. Static pressing sample:

[0053] At present, there is no unified sample preparation method and sample size in the industry for the evaluation of the repair effect of solidified soil. Since the evaluation of the solidification effect in the present invention is mainly the strength and water stability of the solidified soil. Therefore, the present invention refers to the provisions of GB / T50123-2019 "Standard for Geotechnical Test Methods", and the diameter and height of the solidified soil strength sample are 5cm and 10cm respectively, and the static compression sampling method is used for preparation.

[0054] D. Demolding and maintenance:

[0055] After demoulding, the soil samples are quickly tested for size and quality using a vernier caliper and an electronic platform scale. When the diameter and height of the soil samples deviate from the design values ​​by more than 1% or the mass of the soil samples deviate from the design values ​​by more than 1%, the soil samples are discarded and re-sampled. Then, the soil samples that meet the requirements are placed in polyethylene sealed bags (to avoid water loss) and transferred to a standard curing room (relative humidity 98%, temperature 23±1℃) for curing to the design age.

[0056] E. Test determination:

[0057] Examples 1 to 4 and Comparative Examples 1 to 4 were subjected to unconfined compression tests at curing ages of 7d, 14d, and 28d, respectively, according to GB / T 50123-2019 "Standard for Geotechnical Test Methods", and immersed in distilled pure water at 27 days, and continued to be cured for 24h for water stability test.

[0058] Example 1

[0059] A roadbed filler for treating tunnel excavation waste soil based on a curing agent comprises the following components: 420 parts of tunnel waste soil, 23 parts of magnesium slag, 3 parts of fly ash, 2.7 parts of carbide slag, 0.3 parts of desulfurized gypsum, 8 parts of steel slag powder, and 5 parts of magnesium aluminum carbonate hydrotalcite.

[0060] Example 2

[0061] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 420 parts of abandoned soil from tunneling, 27 parts of magnesium slag, 3 parts of fly ash, 0.9 parts of carbide slag, 0.1 parts of desulfurized gypsum, 6 parts of steel slag powder, and 5 parts of magnesium aluminum carbonate hydrotalcite.

[0062] Example 3

[0063] A roadbed filler for treating tunnel excavation waste soil based on a curing agent comprises the following components: 420 parts of tunnel waste soil, 25 parts of magnesium slag, 4 parts of fly ash, 1.8 parts of carbide slag, 0.2 parts of desulfurized gypsum, 7 parts of steel slag powder, and 4 parts of magnesium aluminum carbonate hydrotalcite.

[0064] Example 4

[0065] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 420 parts of abandoned soil from tunneling, 27 parts of magnesium slag, 5 parts of fly ash, 0.9 parts of carbide slag, 0.1 parts of desulfurized gypsum, 6 parts of steel slag powder, and 3 parts of magnesium aluminum carbonate hydrotalcite.

[0066] Example 5

[0067] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 525 parts of abandoned soil from tunneling, 25 parts of magnesium slag, 4 parts of fly ash, 1.8 parts of carbide slag, 0.2 parts of desulfurized gypsum, 7 parts of steel slag powder and 4 parts of magnesium aluminum carbonate hydrotalcite.

[0068] Example 6

[0069] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 350 parts of abandoned soil from tunneling, 25 parts of magnesium slag, 7 parts of fly ash, 1.8 parts of carbide slag, 0.2 parts of desulfurized gypsum, 7 parts of steel slag powder and 4 parts of magnesium aluminum carbonate hydrotalcite.

[0070] Comparative Example 1

[0071] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 420 parts of abandoned soil from tunnel and 25 parts of magnesium slag.

[0072] Comparative Example 2

[0073] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 420 parts of abandoned soil from tunnel and 21 parts of slaked lime.

[0074] Comparative Example 3

[0075] A roadbed filler for treating abandoned soil from tunnel excavation based on a curing agent comprises the following components: 450 parts of abandoned soil from tunneling, 25 parts of magnesium slag, 4 parts of fly ash, 1.8 parts of carbide slag, 0.2 parts of desulfurized gypsum and 7 parts of steel slag powder.

[0076] Comparative Example 4

[0077] A roadbed filler for treating tunnel excavation waste soil based on a curing agent and a preparation process thereof, comprising the following components: 450 parts of tunnel waste soil, 25 parts of magnesium slag, 4 parts of fly ash, 1.8 parts of carbide slag, 0.2 parts of desulfurized gypsum, 7 parts of steel slag powder, and 30 parts of magnesium aluminum carbonate hydrotalcite.

[0078] Table 2 Test results

[0079]

[0080] The test results are shown in Table 2. The curing time has an extremely obvious effect on the strength improvement. When the amount of carbide slag remains unchanged, the addition of fly ash can significantly improve the early strength. The unconfined compressive strength of 0d to 14d increases rapidly, while the increase from 14d to 28d is relatively slow. In addition, with the addition of fly ash, the overall strength of the solidified soil has been improved compared with the single addition of carbide slag, but the more fly ash, the better. Many research results also show that the amount of magnesium slag is still a decisive factor, and the test results are consistent with this.

[0081] In general, the present application makes full use of the high content of sulfate in the tunnel waste residue. In the solidification process of the tunnel waste residue, due to the dual excitation of sulfate and carbide slag, magnesium slag reacts with steel slag and fly ash to generate key hydrated magnesium aluminosilicate (MASH) and hydrated calcium aluminosilicate (CASH) gels. The mesh structure formed by these gels significantly enhances the mechanical properties of the soil. Further stability comes from the reaction between these hydration products and the adsorbent magnesium aluminum carbonate hydrotalcite. In the reaction with magnesium aluminum carbonate hydrotalcite, hydrated magnesium aluminosilicate and hydrated calcium aluminosilicate exchange and synergistic reaction with the cations in magnesium aluminum carbonate hydrotalcite to form a stable phase, which includes but is not limited to ettringite (AFt), hydrated magnesium sulfate and layered double hydroxide (LDHs). The amount of these stable phases generated is related to factors such as reaction conditions and material ratios. Generally, under optimized reaction conditions, the amount of calcium sulfonate generated accounts for 15% to 25%, the amount of hydrated magnesium sulfate generated accounts for 5% to 10%, the amount of magnesium sulfate aluminum hydrotalcite formed accounts for 1% to 3%, and the rest are common hydration gel products such as hydrated calcium silicate and hydrated calcium silicate aluminate. The formation of these stable phases further consolidates the structure of the solidified soil, improves its compressive strength, crack resistance and long-term durability. Among them, when the amount of calcium sulfonate generated is too much, the volume expansion may occur inside the material, thereby causing the risk of cracking or deformation. This is because calcium sulfonate absorbs water and expands during the hydration process. Excessive generation may cause increased internal stress of the material, thereby reducing its overall stability and durability. In addition, too much calcium sulfonate will occupy a large amount of pore space in the material, thereby reducing the generation of other beneficial hydration products and affecting the comprehensive performance of the material. If the amount of calcium sulfonate generated is too small, the sulfate stability of the material may be insufficient, and the problem of structural degradation is prone to occur in a sulfur-containing environment, resulting in a decrease in the ability to resist sulfate erosion, thereby shortening the service life of the material. Excessive production of hydrated magnesium sulfate will affect the chemical stability of the material, especially in a high humidity environment, where dissolution or migration may occur, leading to instability in the internal structure of the material. On the contrary, if too little hydrated magnesium sulfate is produced, the durability of the material may not be sufficient, especially in a sulfate corrosion environment, where the material may be damaged faster. Excessive production of magnesium aluminum sulfate hydrotalcite will make the structure of the material too dense, thereby reducing its water permeability and gas diffusion, affecting the construction performance of the material. If the production of magnesium aluminum sulfate hydrotalcite is insufficient, the sulfate ions in the material may not be fully stabilized, resulting in a decrease in the durability of the material in a sulfate corrosion environment.

[0082] like Figure 2As shown, the hydration product contains 1% to 3% of magnesium aluminum sulfate hydrotalcite, 10% to 15% of ettringite, 5% to 10% of hydrated magnesium sulfate, and the rest is gelling substances such as CASH and MASH. In addition, the generation of macropores in the hydration product is relatively small, and the pore diameter is less than 0.1 μm, so as to ensure the density and impermeability of the material, thereby improving its long-term performance.

[0083] In addition, pyrite cuttings promoted the FeS 2 The hydrolysis of ions produces more sulfate ions, which in turn produces more calcium vanadate and Friedel salt. At the same time, the SiO 2 The vitreous structure decomposes and generates more CAH and CASH structures. These hydration products are gelled together, significantly improving the strength of the solidified soil and reducing the porosity. The strength at 28 days is about 13MPa, far exceeding the strength of traditional lime-based solidifiers by more than 10 times.

[0084] In terms of environmental safety, the adsorption capacity of magnesium aluminum carbonate hydrotalcite for sulfate ions is subject to the different media. In aqueous solution, magnesium aluminum carbonate hydrotalcite effectively adsorbs sulfate ions through ion exchange capacity, but in soil, the adsorption process is more difficult because sulfate ions are physically or chemically bound by soil particles. The addition of carbide slag can increase the pH value of the soil solution through its strong alkalinity, destroy the soil particles' binding to sulfate ions, thereby enhancing the accessibility of sulfate ions and improving the adsorption effect.

[0085] The effect of particle size on hydration products cannot be ignored. Materials with smaller particle sizes have a larger specific surface area, which helps accelerate the hydration reaction and uniformly generate hydration products, reduce porosity, and enhance the overall strength and stability of the material. Small particle size materials have a larger specific surface area and are more likely to form uniform CASH and MASH gels in a high alkalinity environment, further promoting the formation of other stable phases, such as ettringite and layered double hydroxides, enhancing the durability and corrosion resistance of the material.

[0086] In summary, the sulfate activation of carbide slag and tunnel waste soil, the composite reaction of magnesium slag, steel slag and fly ash, and the stability contribution of magnesium aluminum carbonate hydrotalcite have jointly improved the mechanical properties and environmental stability of the solidified soil. The synergistic effect of these factors ensures the comprehensive improvement of the solidified soil in terms of strength and environmental safety.

[0087] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0088] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A roadbed filler for treating salinized loess abandoned from tunnel excavation based on a curing agent, comprising tunnel waste residue, a curing agent and water, characterized in that: The curing agent comprises 23-27 parts of magnesium slag, 3-5 parts of fly ash, 1-3 parts of activator, 6-8 parts of reinforcing agent, and 3-5 parts of adsorbent; The tunnel waste contains chloride ions and sulfate ions, c(SO4 2- ) / c(Cl - )>2.

2. The roadbed filler according to claim 1, characterized in that: The total amount of soluble salt in the tunnel waste is 3.0% to 3.1%, the total amount of chloride ions is 0.20% to 0.30%, and the concentration of sulfate ions is 1.10% to 1.30%.

3. The roadbed filler according to claim 2, characterized in that: The adsorbent is magnesium aluminum carbonate hydrotalcite.

4. The roadbed filler according to claim 3, characterized in that: The activator is a mixture of carbide slag and desulfurized gypsum, with a mass ratio of 9 to 10:1; the reinforcing agent is steel slag powder.

5. The roadbed filler according to claim 4, characterized in that: The roadbed filler is solidified by a solidifying agent. Among the solidified products, the amount of ettringite is 15% to 25%, the amount of hydrated magnesium sulfate is 5% to 10%, the amount of magnesium aluminum sulfate hydrotalcite is 1% to 3%, and the rest is hydrated gelled products.

6. The roadbed filler according to claim 5, characterized in that: The dry mass ratio of the tunnel waste slag to the curing agent is 1:0.08-0.12, and the moisture content of the tunnel waste slag is controlled at 15%-16%.

7. The roadbed filler according to claim 6, characterized in that: The particle size gradation of the tunnel waste slag is as follows: 19% to 20% of the tunnel waste slag with a particle size below 0.005mm, 77% to 78% of the tunnel waste slag with a particle size of 0.005mm to 0.075mm, and 2% to 3% of the tunnel waste slag with a particle size of 0.075mm to 2mm.

8. The roadbed filler according to claim 7, characterized in that: The 7d unconfined compressive strength of the roadbed filler is >1.70MPa; the 28d unconfined compressive strength is >7.84MPa; the water stability coefficient is 70% to 80%.

9. The roadbed filler according to claim 8, characterized in that: The sulfate ion leaching concentration of the roadbed filler is 1701 mg / L to 1758 mg / L.

10. A method for preparing the roadbed filler according to any one of claims 1 to 9, characterized in that: The steps include: The tunnel waste soil, curing agent and water are mixed and then molded and cured in sequence. The dry mass ratio of the tunnel waste soil to the curing agent is 1:0.08-0.12, and the moisture content of the tunnel waste soil is controlled at 15%-16%. The curing method is constant temperature and humidity curing to obtain a roadbed filler.

Citation Information

Patent Citations

  • Curing agent for reinforcing and treating soft soil foundation constructed at low temperature and preparation method thereof

    CN103979914A

  • All-solid waste filling material and preparation method thereof

    CN114940600A

  • All-solid waste soil stabilizer for stabilizing saline soil and preparation method of all-solid waste soil stabilizer

    CN117088626A

  • Method for preparing ceramic water permeable brick from tunnel waste slag

    CN117342857A

  • Solidified agent composition

    KR1020130122171A

Cited By

  • Curing agent, tunnel waste slag regenerated low-permeability material based on curing of multiple solid wastes and preparation method of tunnel waste slag regenerated low-permeability material

    CN119528528A

  • A solidifying agent, a tunnel waste regeneration low-permeability material based on solid waste solidification and a preparation method thereof

    CN119528528B