High-strength cement-based composite material and preparation method thereof

Ceramic sand is prepared by sintering electroplating sludge with construction waste, and combined with other materials, and using pre-wetted ceramic sand as internal curing agent, the shrinkage and deformation problem of high-strength cement matrix is ​​solved, and high strength and high durability are achieved and low-cost cement-based composite materials, extending the service life of the structure.

CN118930174AInactive Publication Date: 2024-11-12ZHEJIANG GUANGTIAN COMPONENT CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411003504.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High-strength cement matrix has significant volume stability problems during the process of increasing strength, resulting in large shrinkage and deformation and cracking of the matrix, thereby reducing the service life of the structure.

Method used

Ceramic sand is prepared by mixing electroplating sludge with construction slag, and combined with materials such as silicate cement, silica fume and blast furnace slag. Pre-wetted ceramic sand is used as internal curing agent to reduce the water-gluing ratio and control the water. Reduce shrinkage deformation.

Benefits of technology

The preparation of high-strength and high-durability cement-based composite materials is realized, which reduces the preparation cost of materials, reduces shrinkage and deformation, improves compactness and structural strength, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930174A_ABST
    Figure CN118930174A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength cement-based composite material and a preparation method thereof.The preparation method comprises the steps that S1, electroplating sludge and building residue soil are prepared, mixed and sintered, pottery sand is obtained, and the pottery sand comprises SiO2, Al2O3 and Fe2O3; s2, Portland cement, silica fume and blast furnace slag are mixed and stirred, and a mixed material is obtained; adding river sand into the mixed material, and further stirring; s3, pre-wetted pottery sand, a water reducing agent and part of water are added into the mixed material stirred in the step S2, and stirring continues; and S4, adding the residual water into the mixed material, and stirring to obtain the high-strength cement-based composite material. The invention also provides components and a ratio of the composite material. According to the invention, the problem of shrinkage of a high-strength cement matrix along with strength improvement in the prior art is solved, the problems of cracking and shortened service life of the shrunk concrete matrix are solved, and the high-strength cement matrix has relatively high commercial value and popularization value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of building materials, and in particular to a high-strength cement-based composite material and a preparation method thereof. Background Art

[0002] Industrial development is usually accompanied by the generation of a large amount of wastewater, which needs to be treated to meet environmental requirements before it can be discharged by the factory. Among them, the sludge after treatment such as electroplating wastewater, pickling wastewater and municipal wastewater contains a large amount of heavy metals. This study refers to this type of sludge as electroplating sludge.

[0003] High Strength Cementitious Matrix (HSCM) is popular in the field of contemporary building materials due to its high strength, high toughness and high durability. HSCM uses a large amount of micro-aggregates, reduces the water-cement ratio, and applies the close packing theory to improve the internal structure of concrete and reduce internal defects. The use of these materials has greatly increased the production cost of HSCM, which is not conducive to the widespread promotion of HSCM. In addition, as the strength of concrete increases, its own shrinkage problem becomes more and more serious, and can even reach 5 to 15 times that of ordinary concrete, and there is a significant volume stability problem. When the shrinkage deformation is large and the ability to resist deformation is weak, the matrix will crack and damage, allowing harmful substances to invade the interior of the concrete, accelerate the deterioration of the concrete and corrode the steel bars, thereby causing the decline of material performance and reducing the service life of the structure. Therefore, the shrinkage problem of HSCM has attracted widespread attention. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a high-strength cement-based composite material, so as to solve the shrinkage problem caused by the increase of strength of the cement matrix prepared by the conventional preparation method, as well as the cracking and reduced life of the concrete matrix after shrinkage, and to provide a method for preparing a high-strength cement-based composite material with simple operation and low preparation cost.

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a high-strength cement-based composite material, comprising the following steps:

[0006] S1: mixing electroplating sludge with construction waste and sintering them to obtain pottery sand;

[0007] S2: Mix 20-40 parts (by mass, the same below) of Portland cement, 2-10 parts of silica fume and 2-20 parts of blast furnace slag, and then add 26-50 parts of river sand and stir to mix;

[0008] S3: adding 12-24 parts of pottery sand, 0.8-1 parts of water reducing agent and 10-18 parts of water obtained in step S1 to the mixed material obtained in step S2, and stirring to obtain a high-strength cement-based composite material.

[0009] In a possible implementation, in step S1, the mass ratio of electroplating sludge to construction waste is 1:(2-3), and the sintering temperature is 1200-1800°C.

[0010] In a possible implementation, in step S3, the ceramic sand is pre-wetted by soaking the ceramic sand in water in advance.

[0011] In the above operation of the present invention, by pre-immersing the pottery sand in water, the phenomenon of strength reduction that may be caused by the introduction of additional water is avoided.

[0012] In the above operation of the present invention, the ceramic sand is soaked in water one day in advance and is ready for use. This pre-wetting treatment method can store more water inside the ceramic sand, so it plays the role of an internal curing agent after the cement matrix is ​​subsequently added.

[0013] In the above preparation method of the present invention, the ceramic sand is prepared by controlling the electroplating sludge and the construction waste soil to be calcined at a high temperature of 1200°C, and is used in a high-strength cement matrix to reduce its shrinkage performance and reduce the preparation cost; secondly, the cement, silica fume and blast furnace slag in the above raw materials are used as fine powders to participate in the hydration reaction and also play a dense filling role; the ceramic sand prepared by high-temperature sintering of the electroplating sludge and the construction waste soil has the characteristics of being porous and can absorb enough water in advance, and can be used as an internal curing agent; in fact, after the pre-wet ceramic sand is added to the cement matrix, it can play the role of a "water reservoir", and the water storage capacity is the amount of pre-absorption of the ceramic sand. With the continuous hydration of the cementitious material, the humidity inside the matrix is ​​reduced, and the water stored in the ceramic sand can be gradually released to promote further hydration. For a high-strength cement matrix with a low water-cement ratio, this is obviously conducive to increasing the humidity inside the matrix, thereby reducing the internal capillary tension and reducing shrinkage deformation. Compared with the method without pre-storing water, this method stores part of the water inside the ceramic sand, the actual mixing water amount is reduced, and the water involved in the early hydration is reduced, so the early hydration process is slowed down.

[0014] Moreover, the combination of the above-mentioned components in the optimal ratio is conducive to promoting further hydration of the cementitious material and giving full play to its activity. At the same time, it can reduce the porosity of the matrix, improve the density, and help improve the strength and durability. At the same time, the addition of ceramic sand can also reduce the shrinkage deformation of the high-strength cement matrix.

[0015] In a possible implementation manner, the ceramic sand prepared in step S1 contains SiO2, Al2O3 and Fe2O3, and the total mass proportion of SiO2, Al2O3 and Fe2O3 is more than 80%.

[0016] In the actual application process of the ceramic sand of the present invention, when the total mass of SiO2, Al2O3, and Fe2O3 is less than 70%, the ceramic sand has no potential activity and only plays a filling role in the matrix. When the total mass of the three reaches more than 80%, the effect of its potential activity is better and can play a greater role.

[0017] In a possible implementation, the high-strength cement-based composite material includes: 28 parts of Portland cement, 10 parts of silica fume, 11 parts of blast furnace slag, 27 parts of river sand, 24 parts of pottery sand, 1 part of water reducer, and 18 parts of water.

[0018] By further optimizing the raw material ratio of the high-strength cement-based composite material of the present invention, the strength of the final composite material is further improved.

[0019] In a possible implementation, the pottery sand prepared in step S1 contains the following components: 50-60 parts of SiO2, 20-25 parts of Al2O3, 4-6 parts of Fe2O3, 5-7 parts of CaO, 2-4 parts of MgO, 2-4 parts of K2O, 0.5-1.5 parts of SO3, 0.01-0.05 parts of P2O5, 0.3-0.8 parts of TiO2, and 3-5 parts of ZnO.

[0020] After the various components in step S2 of the present invention are compounded and combined, it is beneficial to promote the further hydration of the cementitious material, give full play to its activity, and reduce the porosity of the matrix, improve the compactness, and help improve the strength and durability. At the same time, the addition of pottery sand can also reduce the shrinkage deformation of the high-strength cement matrix. At the same time, the present invention also further synergistically improves the structural strength of the final product through the preferred operation of the above steps.

[0021] The fineness of the ceramic sand prepared in step S1 is 2-3, and the apparent density is 1.3×10 3 -1.6×10 3 kg / m3.

[0022] In a possible implementation, in step S3, the particle size of the ceramic sand is greater than or equal to 1.18 mm.

[0023] In the above embodiment of the present invention, coarse pottery sand with the above particle size is used as the pottery sand in the raw material of the present invention. Pottery sand is a lightweight granular material with many tiny pores and gaps inside. Since the coarse pottery sand has a large particle size, more water can be stored in advance. After being added to the cement matrix, it can better play the role of an internal curing agent, which is beneficial to reduce shrinkage deformation and promote further hydration of cementitious materials. However, fine pottery sand with a particle size of less than 1.18 mm has a small sand particle size, limited pre-water storage, limited internal curing effect, and a small degree of shrinkage reduction.

[0024] In a possible implementation, the silicate cement is P II 52.5 silicate cement, and the water reducer is a polycarboxylic acid type water reducer.

[0025] The present invention adopts polycarboxylic acid water reducer as the water reducer. Compared with naphthalene sulfonate water reducer and melamine water reducer, the polycarboxylic acid water reducer with the same dosage contains many small hydrophilic functional groups such as carboxyl groups, sulfonic acid groups, hydroxyl groups, etc., has strong adsorption of cement particles and high dispersibility. After being added to the mortar, the microstructure of the hydration product is denser, the interface structure is good, and higher strength is exhibited.

[0026] In one possible embodiment, the silicate cement has a loss on ignition of less than 1%, a CaO content of 69.9%, a SiO2 content of 15.8%, an Al2O3 content of 4.3%, a particle size of less than 100 μm, a median particle size of 14.6 μm, and an apparent density of 3.042×10 3 kg / m 3 The silica fume has a loss on ignition of <1%, a CaO content of 1.1%, a SiO2 content of 87.7%, an Al2O3 content of 0.5%, a particle size of less than 12 μm, a median particle size of 5.1 μm, and an apparent density of 2.298×10 3 kg / m 3 The blast furnace slag has a loss on ignition of <1%, a CaO content of 1.1%, a SiO2 content of 26.9%, an Al2O3 content of 12.7%, a particle size of less than 400 μm, a median particle size of 10.3 μm, and an apparent density of 2.860 × 10 3 kg / m 3 .

[0027] In a possible implementation, the particle size of the river sand is less than 1.26 μm.

[0028] In a possible implementation, in step S1 and step S2, the stirring condition is: stirring at a speed of 50-100 rpm for 60 s; in step S3 and step S4, the stirring condition is: stirring at a speed of 100-150 rpm for 120 s.

[0029] In the above stirring conditions of the present invention, a stirring speed that is slow at first and then fast is adopted. Since the raw materials are in a powder state at the beginning, stirring too fast will easily cause the powder to be spilled out. Therefore, a stirring speed of 50-100rpm is adopted. After adding water, the raw materials will agglomerate. The raw materials will not spill out due to stirring too fast. Therefore, a stirring speed of 100-150rpm is adopted. By controlling the stirring time and speed to be within the above range of the present invention, it is beneficial to improve the bulk density and compactness of the mixture.

[0030] Another technical problem to be solved by the present invention is to provide a high-strength cement-based composite material to solve the shrinkage problem caused by the increase in strength of the high-strength cement matrix in the prior art, as well as the cracking and reduced life of the concrete matrix after shrinkage. In order to overcome the above defects of the prior art, the present invention provides a high-strength cement-based composite material.

[0031] In order to solve the above technical problems, the present invention provides a high-strength cement-based composite material, and the high-strength cement-based composite material is prepared by the above-mentioned preparation method.

[0032] Compared with the prior art, the high-strength cement-based composite material provided by the present invention has the following advantages: the high-strength cement-based composite material provided by the present invention can realize the resource recycling of electroplating sludge and construction waste, is healthy and environmentally friendly, has excellent mechanical properties, small shrinkage deformation, delayed hydration heat, reduced porosity, and good durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a comparison curve of the autogenous shrinkage within 90 days of the cement matrix of Examples 1 and 2 and the cement matrix of Comparative Examples 1 / 2 / 3;

[0034] Figure 2 The temperature and humidity diagram of the cement matrix of Examples 1 and 2 and the cement matrix of Comparative Examples 1 / 2 / 3 under 20°C environmental conditions is 100mm×100mm×100mm test block;

[0035] Figure 3 It is a comparison diagram of the hydration heat curves of the cement matrices of Examples 1 and 2 and the cement matrices of Comparative Examples 1 / 2 / 3;

[0036] Figure 4 This is the curve of the cumulative proportion of ceramic sand particle size;

[0037] Figure 5 Interface images under SEM scanning electron microscope, where (a) is river sand-slurry interface, and (b) is ceramic sand-slurry interface. DETAILED DESCRIPTION

[0038] First, it should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the embodiments of the present application, and are not intended to limit the protection scope of the embodiments of the present application. Those skilled in the art can make adjustments as needed to adapt to specific applications. In the following and above contents of the present invention, "parts" are all mass parts.

[0039] The present invention provides a method for preparing a high-strength cement-based composite material, comprising the following steps:

[0040] S1: mixing electroplating sludge with construction waste and sintering them to obtain pottery sand;

[0041] S2: Mix 20-40 parts of Portland cement, 2-10 parts of silica fume and 2-20 parts of blast furnace slag, and then add 26-50 parts of river sand and stir to mix;

[0042] S3: adding 12-24 parts of pottery sand, 0.8-1 parts of water reducing agent and 10-18 parts of water obtained in step S1 to the mixed material obtained in step S2, and stirring to obtain a high-strength cement-based composite material.

[0043] As a preferred solution, in step S1, the mass ratio of electroplating sludge to construction waste soil is 1:(2-3), and the sintering temperature is 1200-1800°C.

[0044] As a preferred solution, the components of the ceramic sand prepared in step S1 include SiO2, Al2O3 and Fe2O3, and the total mass proportion of SiO2, Al2O3 and Fe2O3 is more than 80%.

[0045] As a preferred solution, the high-strength cement-based composite material includes: 28 parts of silicate cement, 10 parts of silica fume, 11 parts of blast furnace slag, 27 parts of river sand, 24 parts of pottery sand, 1 part of water reducer, and 18 parts of water.

[0046] By further optimizing the raw material ratio of the high-strength cement-based composite material of the present invention, the strength of the final composite material is further improved.

[0047] As a preferred solution, the pottery sand prepared in step S1 contains the following components: 50-60 parts of SiO2, 20-25 parts of Al2O3, 4-6 parts of Fe2O3, 5-7 parts of CaO, 2-4 parts of MgO, 2-4 parts of K2O, 0.5-1.5 parts of SO3, 0.01-0.05 parts of P2O5, 0.3-0.8 parts of TiO2, and 3-5 parts of ZnO.

[0048] The fineness of the ceramic sand prepared in step S1 is 2-3, and the apparent density is 1.3×10 3 -1.6×10 3 kg / m3.

[0049] As a preferred solution, in step S3, the particle size of the ceramic sand is greater than or equal to 1.18 mm.

[0050] In the above preferred embodiment of the present invention, coarse pottery sand with the above particle size is used as the pottery sand in the raw material of the present invention. Since the coarse pottery sand has a larger particle size, more water can be stored in advance. After being added to the cement matrix, it can better play the role of an internal curing agent, which is beneficial to reducing shrinkage deformation and promoting further hydration of the cementitious material; while fine pottery sand with a particle size of less than 1.18 mm has a small sand particle size, limited pre-water storage capacity, limited internal curing effect, and a small degree of shrinkage reduction. Although small-particle pottery sand is beneficial to improving gradation distribution, increasing the bulk density of the mixture, reducing the matrix porosity, and thereby improving the early strength, since the purpose of the present invention is to reduce shrinkage, the addition of coarse pottery sand can further improve the shrinkage problem existing in the prior art.

[0051] Figure 4 The cumulative proportion curve of the ceramic sand particle size shows that the fine ceramic sand below 1.18 mm accounts for a large proportion of the sintered ceramic sand. However, ceramic sand with too large a particle size will become a weak link in the high-strength cement matrix. Therefore, the particle size of the coarse ceramic sand in the present invention is preferably 1.18-5 mm. Figure 4 As shown, the more preferred value is 1.18 mm, the inflection point of the curve, which can store more water without excessively affecting the particle size curve distribution of the raw materials.

[0052] As a preferred solution, in step S3, the ceramic sand is pre-wetted by soaking the ceramic sand in water in advance.

[0053] As a preferred solution, the silicate cement is P II 52.5 silicate cement, and the water reducer is a polycarboxylic acid type water reducer.

[0054] As a preferred solution, the silicate cement has a loss on ignition of less than 1%, a CaO content of 69.9%, a SiO2 content of 15.8%, an Al2O3 content of 4.3%, a particle size of less than 100 μm, a median particle size of 14.6 μm, and an apparent density of 3.042×10 3 kg / m 3 The silica fume has a loss on ignition of <1%, a CaO content of 1.1%, a SiO2 content of 87.7%, an Al2O3 content of 0.5%, a particle size of less than 12 μm, a median particle size of 5.1 μm, and an apparent density of 2.298×10 3 kg / m 3The blast furnace slag has a loss on ignition of <1%, a CaO content of 1.1%, a SiO2 content of 26.9%, an Al2O3 content of 12.7%, a particle size of less than 400 μm, a median particle size of 10.3 μm, and an apparent density of 2.860 × 10 3 kg / m 3 .

[0055] As a preferred solution, the particle size of the river sand is less than 1.26 μm.

[0056] As a preferred solution, in step S1 and step S2, the stirring condition is: stirring at a speed of 50-100 rpm for 60 s; in step S3 and step S4, the stirring condition is: stirring at a speed of 100-150 rpm for 120 s.

[0057] The present invention also provides a high-strength cement-based composite material, which is prepared by the above-mentioned preparation method.

[0058] In order to explain the above embodiments, the present invention further proposes the following embodiments to explain the above technical solution. In the following content of the present invention, fine pottery sand is pottery sand with a particle size of less than 1.18 mm, and coarse pottery sand is pottery sand with a particle size of 1.18-5 mm:

[0059] Embodiment 1:

[0060] The high-strength cement matrix of this embodiment is composed of 28 parts of P II 52.5 silicate cement, 10 parts of silica fume, 11 parts of blast furnace slag, 38 parts of river sand, 24 parts of coarse pottery sand, 0.8 parts of water reducer, and 18 parts of water;

[0061] The preparation method of the cement matrix comparative example comprises:

[0062] S1: preparing electroplating sludge and construction waste soil, mixing them, and sintering them at a temperature of 1200° C. to obtain pottery sand;

[0063] The composition of the ceramic sand is calculated by mass ratio, including: SiO2: 57.45%; Al2O3: 20.85%; FE2O3: 4.92%; CaO: 6.09%; MgO: 2.64%; K2O: 2.34%; SO3: 0.96%; P2O5: 0.03%; TiO2: 0.50%; ZnO: 4.23%; Loi: 0.97%; wherein the total mass proportion of SiO2, Al2O3 and Fe2O3 is 83.22%;

[0064] S2: 28 parts of P II 52.5 silicate cement, 10 parts of silica fume, and 11 parts of blast furnace slag were mixed and stirred at a speed of 60 rpm for 60 seconds to obtain a mixed material;

[0065] Add 38 parts of river sand to the mixture in step S1 and stir it for 60 seconds at a speed of 60 rpm;

[0066] S3: one day before molding, pre-wet the coarse ceramic sand with half the amount of water in the ratio table to store enough water inside the ceramic sand; add the pre-wetted ceramic sand, water reducer (polycarboxylic acid type water reducer, solid content 35%) and part of the water (1 / 4 of the total water volume) to the mixed material after stirring in step S2, and continue stirring at a speed of 120 rpm for 120 seconds;

[0067] The remaining water (1 / 4 of the total water volume) was added to the mixed material after the treatment in step S3, and stirred at a rotation speed of 120 rpm for 120 seconds to obtain a cement matrix comparative example.

[0068] The silicate cement has a loss on ignition of less than 1%, a CaO content of 69.9%, a SiO2 content of 15.8%, an Al2O3 content of 4.3%, a particle size of less than 100 μm, a median particle size of 14.6 μm, and an apparent density of 3.042×10 3 kg / m 3 The ignition loss of the silica fume is less than 1%, the CaO content is 1.1%, the SiO2 content is 87.7%, and the Al2O3 content is 0.5%. The particle size is less than 12μm, the median particle size is 5.1μm, and the apparent density is 2.298×10 3 kg / m 3 The ignition loss of the blast furnace slag is less than 1%, the CaO content is 1.1%, the SiO2 content is 26.9%, and the Al2O3 content is 12.7%. The particle size is less than 400 μm, the median particle size is 10.3 μm, and the apparent density is 2.860×10 3 kg / m 3 .

[0069] The particle size of the river sand is less than 1.26 μm, the fineness is 2.27±0.2, and the apparent density is (1.606±0.2)×10 3 kg / m 3 .

[0070] The ceramic sand is made by high-temperature sintering of electroplating sludge and construction waste in a ratio of 1:3, and the fineness of the ceramic sand is 2.77±0.2, and the apparent density is (1.518±0.2)×10 3 kg / m 3 .

[0071] The preparation method of the high-strength cement-based composite material of Example 2 is the same as that of Example 1, except that the formula of the cement matrix comparative example is different, specifically:

[0072] Embodiment 2:

[0073] The high-strength cement matrix of this embodiment is composed of 28 parts of P II 52.5 silicate cement, 10 parts of silica fume, 11 parts of blast furnace slag, 38 parts of river sand, 12 parts of coarse pottery sand, 0.8 parts of water reducer, and 18 parts of water.

[0074] Embodiment 3:

[0075] The preparation method of the high-strength cement-based composite material of Example 3 is similar to that of Example 1, except that in step S1, the sintering temperature is 1500° C.; and the formula of the cement matrix of Example 3 is different, specifically:

[0076] The high-strength cement matrix of this embodiment is composed of 20 parts of P II 52.5 silicate cement, 2 parts of silica fume, 2 parts of blast furnace slag, 26 parts of river sand, 12 parts of coarse pottery sand, 0.8 parts of water reducer, and 10 parts of water.

[0077] Embodiment 4:

[0078] The preparation method of the high-strength cement-based composite material of Example 4 is similar to that of Example 1, except that in step S1, the sintering temperature is 1800° C.; and the formula of the cement matrix of Example 3 is different, specifically:

[0079] The high-strength cement matrix of this embodiment is composed of 40 parts of P II 52.5 silicate cement, 10 parts of silica fume, 20 parts of blast furnace slag, 50 parts of river sand, 24 parts of pottery sand, 1 part of water reducer, and 18 parts of water.

[0080] Comparative Example 1:

[0081] The cement matrix of this comparative example is composed of 28 parts of P II 52.5 Portland cement, 10 parts of silica fume, 11 parts of blast furnace slag, 26 parts of river sand, 24 parts of fine pottery sand, 0.8 parts of water reducer, and 18 parts of water;

[0082] The preparation method of the cement matrix comparative example comprises:

[0083] S1: preparing electroplating sludge and construction waste soil, mixing them, and sintering them at a temperature above 1200°C to obtain pottery sand;

[0084] S2: Mixing and stirring silicate cement, silica fume and blast furnace slag at a rotation speed of 60 rpm for 60 seconds to obtain a mixed material;

[0085] S3: one day before molding, pre-wet the ceramic sand with half the amount of water in the ratio table to store enough water inside the ceramic sand; add the pre-wetted ceramic sand, water reducer (polycarboxylic acid type water reducer, solid content 35%) and part of the water (1 / 4 of the total water volume) to the mixed material after stirring in step S2, continue stirring, and stir at a speed of 120 rpm for 120 seconds;

[0086] S4: adding the remaining water (1 / 4 of the total water volume) to the mixed material after the treatment in step S3, stirring at a rotation speed of 120 rpm for 120 seconds to obtain a cement matrix comparative example.

[0087] The silicate cement has a loss on ignition of less than 1%, a CaO content of 69.9%, a SiO2 content of 15.8%, an Al2O3 content of 4.3%, a particle size of less than 100 μm, a median particle size of 14.6 μm, and an apparent density of 3.042×10 3 kg / m 3 The ignition loss of the silica fume is less than 1%, the CaO content is 1.1%, the SiO2 content is 87.7%, and the Al2O3 content is 0.5%. The particle size is less than 12μm, the median particle size is 5.1μm, and the apparent density is 2.298×10 3 kg / m 3 The ignition loss of the blast furnace slag is less than 1%, the CaO content is 1.1%, the SiO2 content is 26.9%, and the Al2O3 content is 12.7%. The particle size is less than 400 μm, the median particle size is 10.3 μm, and the apparent density is 2.860×10 3 kg / m 3 .

[0088] The particle size of the river sand is less than 1.26 μm, the fineness is 2.27±0.2, and the apparent density is (1.606±0.2)×10 3 kg / m 3 .

[0089] The ceramic sand is made by high-temperature sintering of electroplating sludge and construction waste in a ratio of 1:3, and the fineness of the ceramic sand is 2.77±0.2, and the apparent density is (1.518±0.2)×10 3 kg / m 3 .

[0090] The preparation methods of the cement matrix comparative examples of comparative examples 2-3 are the same as those of comparative example 1, except that the formulas of the cement matrix comparative examples are different, specifically:

[0091] Comparative Example 2:

[0092] The cement matrix of this comparative example consists of 28 parts of P II 52.5 silicate cement, 10 parts of silica fume, 11 parts of blast furnace slag, 38 parts of river sand, 12 parts of fine ceramic sand, 0.8 parts of water reducer and 18 parts of water.

[0093] Comparative Example 3:

[0094] The cement matrix of this comparative example is composed of 28 parts of P II 52.5 silicate cement, 10 parts of silica fume, 11 parts of blast furnace slag, 38 parts of river sand, 0.8 parts of water reducer, and 18 parts of water. This comparative example does not include pottery sand, and other preparation methods are the same as those of comparative example 1.

[0095] The slump and strength tests of the ecological high-strength cement matrix prepared in the above embodiment and comparative example were carried out, and the strength and cost advantages of the embodiment were obtained by cost analysis. The advantages of the optimized ratio in terms of shrinkage reduction were further obtained by analyzing the autogenous shrinkage performance, internal humidity and compressive strength of the embodiment, and the measurement results are shown in Tables 1 and 2.

[0096] Comparative Example 4:

[0097] The preparation method of the cement matrix comparative example of this comparative example is the same as that of Example 1, except that the formula of the cement matrix comparative example is different, specifically:

[0098] The coarse pottery sand used in the comparative example 4 is prepared as follows: S1: electroplating sludge and construction waste are mixed in a mass ratio of 1:1 and sintered at 1200°C to obtain pottery sand; the total mass proportion of SiO2, Al2O3 and Fe2O3 in the prepared pottery sand is 68%.

[0099] Comparative Example 5:

[0100] The preparation method of the cement matrix comparative example of this comparative example is the same as that of Example 1, except that the formula of the cement matrix comparative example is different, specifically:

[0101] The coarse pottery sand used in the comparative example 4 is prepared as follows: S1: electroplating sludge and construction waste are mixed in a mass ratio of 1:1.5 and sintered at 1200°C to obtain pottery sand, in which the total mass proportion of SiO2, Al2O3 and Fe2O3 is 75%.

[0102] Comparative Example 6:

[0103] The preparation method and formulation of the cement matrix of this comparative example are the same as those of Example 1, except that in step S1, the sintering temperature is 2000°C.

[0104] Comparative Example 7:

[0105] The preparation method and formulation of the cement matrix of this comparative example are the same as those of Example 1, except that in step S1, the sintering temperature is 800°C.

[0106] Table 1 Comparison of slump, 28d compressive strength and cost between different embodiments and comparative examples

[0107]

[0108] It can be seen from the above results that, whether comparing Comparative Example 1 / 2 with the Comparative Example or Example 1 / 2 with Comparative Example 3, it can be found through the slump in the above table that the embodiments used in the present invention are superior to all comparative examples, further proving that the product prepared by the embodiments of the present invention has excellent fluidity, and the present invention has high cost performance, and has the advantages of high strength and low cost compared to the proportion of Comparative Example 1 / 2 with fine ceramsite added; and in the comparison between Example 1 / 2 and Comparative Example 1 / 2, Example 1 / 2 with coarse ceramsite added is superior to the embodiment with fine ceramsite added in terms of 28d compressive strength and 28d compressive strength / cost, which also proves that coarse ceramsite is better than fine ceramsite in improving the performance of the high-strength cement matrix prepared by the present invention. Compared with Examples 1-2 of the present invention, the 28d compressive strength / cost of other comparative examples are also mostly lower than that of the embodiments of the present invention: including Comparative Examples 4 / 5, when the total mass proportion of SiO2, Al2O3 and Fe2O3 in the ceramsite is less than 80%, it has a great influence on its slump and 28d compressive strength, which further proves that the present invention can improve the performance of the final product by controlling the total mass proportion of SiO2, Al2O3 and Fe2O3 in the ceramsite to more than 80%; and Comparative Examples 6 / 7, the calcination temperature is outside the scope of the present invention. When the temperature is higher (Comparative Example 6), there is no improvement on the performance, and the preparation cost is further increased. When the temperature is lower (Example 7), the performance of the product cannot be improved. This further proves that the present invention controls the calcination temperature at 1200-1800°C, which plays an extremely important role in controlling costs and improving material properties.

[0109] This also further proves that when the formula components of the cement matrix are within the range defined by the present invention, a cement matrix with higher 28d compressive strength / cost can be obtained.

[0110] Table 2 Comparison of autogenous shrinkage and internal humidity in different embodiments

[0111]

[0112] From the above results, it can be seen that in Comparative Example 3, as a blank comparative example without ceramsite, compared with the ratio without adding ceramic sand, in the group of Comparative Example 1 / 2, it can be seen that the addition of fine ceramic sand can reduce the shrinkage to a certain extent. For example, Comparative Example 1 / 2 can reduce the autogenous shrinkage deformation from 1250με to 781με and 744με, and the effect of continuing to increase the dosage of fine ceramic sand is no longer obvious; and by comparing the Example 1 / 2 group with the Comparative Example 3, it is proved that the addition of coarse ceramic sand can significantly reduce the autogenous shrinkage deformation, such as Example 1 and Example 2 can reduce the autogenous shrinkage deformation. The shrinkage deformation is reduced to 694με and 225με; and as the comparative example 4 / 5 whose total mass of SiO2, Al2O3 and Fe2O3 is less than 80%, although its autogenous shrinkage performance is also improved, it is obviously not as good as that of the examples 1 / 2; similarly, for the comparative examples 6 / 7 with different calcination temperature ranges, the 28d autogenous shrinkage performance of the comparative example 6 is slightly higher than that of the example 1, but its calcination temperature is higher, the actual preparation cost is higher, and the effect is reduced. Due to the insufficient calcination temperature of the comparative example 7, the activity of the pottery sand is insufficient, and the final performance is poor.

[0113] The autogenous shrinkage deformation curves of different comparison ratios can also be found in Figure 1 see from Figure 2 It can also be seen from the internal humidity that with the increase of the amount of pottery sand and the particle size, the internal humidity increases and the capillary tension decreases, thus reducing the shrinkage deformation; Figure 3 It can be seen that with the increase of the amount of clay sand and the increase of particle size, the peak value of hydration heat decreases and there is an obvious peak right shift phenomenon, which shows that the addition of clay sand delays the early hydration reaction and is conducive to reducing the early hydration heat. Compared with fine clay sand, the effect of coarse clay sand is more significant. Figure 5 This is a comparison diagram of the ceramic sand-slurry interface and the river sand-slurry interface in the product obtained in the embodiment of the present invention. It can be seen that the interface between the river sand and the slurry is relatively smooth and has a large gap, while the interface between the ceramic sand and the matrix is ​​uneven and more tightly bonded. In addition to being attributed to the porous nature of the ceramic sand itself, it can also be attributed to the internal curing effect of the ceramic sand, which promotes the further hydration of the nearby gel material, making the structure more compact.

[0114] According to the comparison of the above embodiments and comparative examples, it is further proved that the present invention provides a high-strength cement-based composite material and a preparation method thereof, which solves the shrinkage problem of the high-strength cement matrix caused by the increase of strength in the prior art, as well as the problems of cracking and reduced life of the concrete matrix after shrinkage, and provides a high-strength cement-based composite material with high strength, low cost and high cost performance and a preparation method thereof, and the preparation method is simple, does not require cumbersome operations and complicated equipment, and has high commercial value and promotion value.

[0115] In the description of the embodiments of the present application, it should be noted that in the description of the present application, terms such as "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is only for the convenience of description, and does not indicate or imply that the device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present application.

[0116] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0117] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for preparing a high-strength cement-based composite material, It is characterized in that The following steps are involved: S1: mixing electroplating sludge with construction waste and sintering them to obtain pottery sand; S2: Mix 20-40 parts of Portland cement, 2-10 parts of silica fume and 2-20 parts of blast furnace slag, and then add 26-50 parts of river sand and stir to mix; S3: adding 12-24 parts of pottery sand, 0.8-1 parts of water reducing agent and 10-18 parts of water obtained in step S1 to the mixed material obtained in step S2, and stirring to obtain a high-strength cement-based composite material.

2. The method for preparing the high-strength cement-based composite material according to claim 1, It is characterized in that In the step S1, the mass ratio of electroplating sludge to construction waste soil is 1:2-3, and the sintering temperature is 1200-1800°C.

3. The method for preparing the high-strength cement-based composite material according to claim 2, It is characterized in that The composition of the ceramic sand prepared in step S1 includes SiO 2 、Al 2 O 3 and Fe 2 O 3 , and SiO 2 、Al 2 O 3 and Fe 2 O 3 The total quality accounts for more than 80%.

4. The method for preparing the high-strength cement-based composite material according to claim 3, It is characterized in that The ceramic sand prepared in step S1 contains the following components: SiO 2 50-60 parts, Al 2 O 3 20-25 parts, Fe 2 O 3 4-6 parts, CaO 5-7 parts, MgO 2-4 parts, K 2 O 2-4 parts, SO 3 0.5-1.5 parts, P 2 O 5 0.01-0.05 parts, TiO 2 0.3-0.8 parts, ZnO 3-5 parts.

5. The method for preparing the high-strength cement-based composite material according to claim 2, It is characterized in that The fineness of the ceramic sand prepared in step S1 is 2-3, and the apparent density is 1.3×10 3 -1.6×10 3 kg / m 3 .

6. A method for preparing a high-strength cement-based composite material according to any one of claims 1 to 5, It is characterized in that In step S3, the particle size of the ceramic sand is greater than or equal to 1.18 mm.

7. The method for preparing the high-strength cement-based composite material according to claim 1, It is characterized in that In the step S3, the ceramic sand is pre-wetted by soaking the ceramic sand in water in advance.

8. The method for preparing the high-strength cement-based composite material according to claim 1, It is characterized in that The silicate cement is PII 52.5 silicate cement, and the water reducer is a polycarboxylic acid type water reducer.

9. The method for preparing the high-strength cement-based composite material according to claim 1, It is characterized in that The particle size of the river sand is less than 1.26 μm.

10. A high-strength cement-based composite material, It is characterized in that Prepared by the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Resourceful treatment method for sludge drying, incineration and granulation

    CN112679222A

  • High-crack-resistance light-weight high-strength self-compacting concrete and preparation method thereof

    CN112960952A

  • Application of heavy metal sludge high-temperature treatment slag charge and portland cement-based material containing slag charge

    CN113233806A

  • Internal curing low-shrinkage lightweight aggregate ultra-high performance concrete and preparation method thereof

    CN113321467A

  • Process for preparing novel sludge ceramsite

    CN115028431A