Single-component joint mixture and preparation method thereof

Through the single-component fridge formula, combined with specific proportions and stirring sequence, the problems of complex operation and insufficient anti-alkali performance of two-component fridge are solved, and the effect of simplifying construction and improving the performance of the fridge is achieved.

CN118930193APending Publication Date: 2024-11-12SHANGHAI NIUYUAN IND TRADE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411217403.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing two-component seam caulking agents are complex in operation and are difficult to use in construction sites with large slopes. The surface is prone to scratches. The single-component seam caulking agents, especially the anti-alkali properties, are insufficient.

Method used

The single-component caulking agent formula is adopted, including cement, stone powder, glue powder, premature strength agent, cellulose ether, anti-alkali agent and hydrophobic agent, to improve the strength and caulking agent through specific proportions and stirring sequences. Water performance reduces the risk of pan-alkali.

Benefits of technology

It has achieved simplified construction operations, improved the strength and hydrophobic properties of the joint filler, reduced the risk of alkaline phenomenon, and enhanced the stability and aesthetics of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021944340000111
    Figure BDA0005021944340000111
  • Figure BDA0005021944340000121
    Figure BDA0005021944340000121
  • Figure BDA0005021944340000122
    Figure BDA0005021944340000122
Patent Text Reader

Abstract

The invention relates to the field of building materials, in particular to the field of C04B28 / 00, and specifically relates to a single-component joint mixture and a preparation method thereof. The single-component joint mixture is prepared from the following raw materials: cement, stone powder, rubber powder, an early strength agent, cellulose ether, an alkali efflorescence resisting agent, a water repellent and a mildew preventive. The preparation method comprises the following steps: mixing the stone powder and the water repellent, and stirring for 10-30 minutes; and adding the cement, the rubber powder, the early strength agent, the cellulose ether, the mildew preventive and the alkali efflorescence resistant agent, and mixing and stirring for 30-60 minutes to obtain the concrete. The single-component joint mixture provided by the invention is excellent in hydrophobicity and saltpetering resistance and has an excellent actual use effect, and the preparation method is simple and easy to implement and can be suitable for expanded production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, in particular to the field of C04B28 / 00, and specifically to a single-component caulking agent and a preparation method thereof. Background Art

[0002] Tiles are easy to care for, easy to clean, and have excellent properties such as water resistance and scratch resistance. They have been widely used. However, after long-term use, the surface performance of tiles will inevitably decline to a certain extent. As the material ages or is impacted by external forces, large or small gaps often appear on the surface of tiles, affecting the appearance and product life. Caulking agents are used to fill the gaps of materials such as ceramic tiles and artificial stones. Therefore, they have been widely used in home building materials, commercial building materials and other fields. Currently, the most common caulking agents are generally two-component caulking agents.

[0003] Prior art CN201510875908.1, CN201910105170.9, and CN201910007919.6 all disclose two-component caulking agents. Two-component caulking agents have the advantages of higher hardness, better color retention, waterproof and dustproof, chemical corrosion resistance, wear resistance, and impact resistance, but the operation process of two-component caulking agents is relatively complicated and requires professional mixing equipment and construction tools, which increases the difficulty and technical requirements of construction. In addition, since two-component caulking agents require leveling construction, there are certain requirements for the slope of the construction site, and it is not suitable to implement it when the slope is large, which limits its flexibility of use. Finally, although two-component caulking agents have good durability and aesthetics, their surface is easily scratched, and once scratched, it will affect the overall aesthetics. At present, there are few reports on single-component caulking agents, and even fewer reports on single-component caulking agents with anti-panning alkali properties.

[0004] The prior art 201410559553.0 discloses an anti-efflorescence alkali-resistant facing mortar for exterior walls, which is mainly composed of cement, quartz powder, redispersible latex powder, nano-grade rubber powder, filler, natural sand and additives. After use, it can effectively eliminate the alkali return phenomenon, but its water-reducing performance can be further improved. Summary of the invention

[0005] In order to solve the above technical problems, the first aspect of the present invention provides a one-component caulking agent, the raw materials for preparing the caulking agent include: cement, stone powder, glue powder, early strength agent, cellulose ether, anti-efflorescence agent, water repellent agent, and mildew inhibitor.

[0006] Further preferably, the raw materials for preparing the one-component caulking agent include, by weight: 40-50 parts of cement, 50-60 parts of stone powder, 1-3 parts of glue powder, 0.1-1 parts of early strength agent, 0.1-1 parts of cellulose ether, 0.1-1 parts of anti-efflorescence agent, 0.1-1 parts of water repellent, and 0.1-1 parts of mildew preventer.

[0007] More preferably, the raw materials for preparing the one-component caulking agent include, by weight: 40-45 parts of cement, 52-57 parts of stone powder, 1-2 parts of glue powder, 0.8-1 parts of early strength agent, 0.1-0.2 parts of cellulose ether, 0.1-0.3 parts of anti-efflorescence agent, 0.3-0.6 parts of water repellent, and 0.4-0.5 parts of mildew inhibitor.

[0008] cement

[0009] Preferably, the cement strength grade is 40-65. As an implementable case, the cement strength grades include: 42.5, 42.5R, 52.5, 52.5R, 62.5, and 62.5R.

[0010] Further preferably, the intensity grade of the water washing is 52.5.

[0011] The 52.5 grade cement used in the present invention has the advantages of high early strength, good wear resistance, strong impermeability and erosion resistance; it is suitable for various main projects constructed at low temperature and negative temperature; in addition, the 52.5 grade cement is also suitable for large-volume concrete projects, has high performance stability and color stability, and can be widely used in the preparation of caulking agents; however, the main component of cement is alkaline silicate. As the use time increases, soluble salts and alkalis precipitate in the capillaries to generate crystallization pressure. This pressure is sufficient to cause the concrete to crack, thereby causing the structure to be destroyed and affecting the normal use of the product. Therefore, it is necessary to avoid the occurrence of efflorescence as much as possible.

[0012] Stone powder

[0013] Preferably, the stone powder includes calcium carbonate white stone powder, and the particle size of the calcium carbonate is 100-600 mesh.

[0014] Further preferably, the particle size of the stone powder is 325 mesh. As an implementable case, the stone powder can be selected from Feiteng 325 mesh white stone powder.

[0015] The present invention preferably uses cement of grade 52.5 strength, which can improve the uniformity of the caulking agent, achieve the effect of rapid hardening, and is also beneficial to improving the early strength, frost resistance, wear resistance, and anti-penetration performance. However, its mechanical properties are somewhat different from those of grade 62.5 and grade 62.5R cements. However, due to the high cost of grade 62.5 and grade 62.5R cements, the inventors choose to use stone powder, especially 325-mesh calcium carbonate white stone powder, which can fill the uneven surface of grade 52.5 cement and improve the density and strength of the caulking agent material. However, particles larger than 100 mesh have little effect on the hydration and strength of cement and only serve as fillers. Stone powder that is too fine and smaller than 600 mesh may agglomerate or increase the water demand of cement, complete the hydration process before the slurry hardens, and has no effect on the growth of cement age strength.

[0016] Rubber powder

[0017] Preferably, the rubber powder includes: one of vinyl acetate-ethylene copolymer rubber powder, acrylate-styrene copolymer rubber powder, ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and styrene-butadiene copolymer rubber powder.

[0018] Further preferably, the rubber powder includes ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder. As an implementable case, the rubber powder model is Wacker 8034H.

[0019] The preferred ethylene-vinyl laurate-vinyl chloride copolymer ternary copolymer powder in the present invention has hydrophobicity and can improve the waterproof performance of the material; and the ethylene-vinyl laurate-vinyl chloride copolymer ternary copolymer powder has certain adhesive properties. When used together with 52.5 grade cement and 325 mesh calcium carbonate stone powder, it can improve the bonding ability and tensile resistance of the premixed dry mortar, and further increase the strength of the mortar; in addition, the ethylene-vinyl laurate-vinyl chloride copolymer ternary copolymer powder has no adverse effect on the fluidity, thixotropy and water retention of the material, and ensures the comprehensive performance of the material during use. However, the ethylene-vinyl laurate-vinyl chloride copolymer ternary copolymer powder in the present invention is not easy to use excessively. Although the powder can improve the tensile strength and interfacial bonding tensile strength of the caulking agent and improve the bonding tensile strength between the mortar and the substrate, excessive use may lead to the introduction of too many bubbles, thereby causing the compressive strength to show a downward trend. Therefore, the preferred mass fraction of the powder in the present invention is 1-2 parts.

[0020] Early strength agent

[0021] Preferably, the early strength agent includes: one of calcium chloride, sodium sulfate, gypsum, water glass, sodium aluminate, sodium carbonate, calcium carbonate, calcium formate, sodium fluoride, and triethanolamine.

[0022] Further preferably, the early strength agent is calcium formate; as an implementable case, the calcium formate is purchased from Shandong Fenlian Chemical.

[0023] Calcium formate can significantly accelerate the hardening speed of cement in the sealant, reduce the construction period, and make the concrete coagulate and shape faster; by increasing the early strength of cement-based materials, shortening the time for concrete to reach load capacity, and improving the quality and durability of the building. Under low temperature conditions, calcium formate can prevent the slow setting phenomenon of cement, maintain the normal hardening process of cement, and thus prevent concrete from being damaged by freezing. Therefore, the sealant of the present invention can be used in some severely cold areas. In addition, calcium formate can significantly shorten the initial setting time of concrete, and improve the compactness, durability and impermeability of the product. However, excessive use of calcium formate may have a certain negative impact on the durability of the sealant, increase the risk of cracking of concrete, etc.

[0024] Cellulose ether

[0025] Preferably, the cellulose ether includes: one of anionic cellulose ether, cationic cellulose ether and nonionic ether cellulose ether.

[0026] Further preferably, the cellulose ether is a nonionic cellulose ether, including: one of methyl cellulose ether, hydroxypropyl methyl cellulose ether, hydroxyethyl methyl cellulose ether, and hydroxyethyl cellulose ether; more preferably, the cellulose ether is hydroxyethyl methyl cellulose ether; hydroxyethyl methyl cellulose ether can be purchased from Dow Chemical, model MKX15000PP20.

[0027] Hydroxyethyl methyl cellulose ether contains methoxy groups in its molecules, which can greatly improve the water retention of cement mortar and prevent water loss too quickly, thereby promoting cement hydration and ultimately improving the mechanical properties of the sealant. In addition, hydroxyethyl methyl cellulose ether can also slow down the volatilization rate of water molecules, which helps the cement hydration process and further enhances the strength of the sealant.

[0028] Anti-efflorescence agent

[0029] Preferably, the anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, and a pH value of 8-10 (10% aqueous solution); as an implementable case, the anti-efflorescence agent is Celanese ERA-200.

[0030] In the present invention, the preferred bulk density is 350-550 g / L, the particle size is less than 250 μm, and the pH value is 8-10 (10% aqueous solution), which has a significant effect on inhibiting the primary and secondary efflorescence effects. In addition to reducing the risk of efflorescence, it can also improve the stability of the wet mortar and the surface hydrophobic effect.

[0031] Water repellent

[0032] Preferably, the water repellent comprises an inorganic water repellent and / or an organic water repellent.

[0033] More preferably, the water repellent is an organic water repellent.

[0034] More preferably, the organic hydrophobic agent includes sodium stearate and an organosilicon hydrophobic agent in a mass ratio of 1:(1-3); as an implementable case, the organosilicon hydrophobic agent includes but is not limited to Wacker powder A.

[0035] Sodium stearate is a natural fatty acid salt with good hydrophobicity, which can reduce the water permeability of mortar or concrete under hydrostatic pressure, thereby achieving a water-repellent effect; the silicone water-repellent Wacker powder A can improve the waterproofness and water resistance of cement-based powder coatings, making the products show extremely low water absorption, extremely stain-resistant and long-term durability. The inventors have found that when sodium stearate and silicone water-repellent are compounded in a mass ratio of 1: (1-3), they can work synergistically, and the stearic acid chain and the silicone resin are cross-linked and entangled, further improving the water-repellent performance of the caulking agent in the present invention.

[0036] Antifungal agent

[0037] Preferably, the mildew inhibitor includes one or more of Hoffman Defros M12, Hoffman Defros M6, Hoffman Defros M1, and Hoffman Defros M3.

[0038] Further preferably, the mildewcide includes Hofmann Defros M12.

[0039] In order to improve the mildew-proof storage performance of the caulking agent in the present invention, the present invention preferably uses the mildew-proof agent Hofmann Defros M12, which has the characteristics of high temperature and high humidity resistance and effectively inhibits the growth of bacteria, fungi and algae. At the same time, the mildew-proof agent Hofmann Defros M12 in the present invention can also improve the hydrophobicity of the caulking agent to a certain extent, and the comprehensive application performance of the product is more excellent.

[0040] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0041] S1. Mix the stone powder and water repellent and stir for 10-30 minutes;

[0042] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30-60 minutes.

[0043] The product of the invention is a single-component powder without solvent, and can be directly mixed and stirred with water in a mass ratio of 100:(30-35) during construction.

[0044] Compared with the preparation method of mixing and stirring all raw materials at a time, the present invention first mixes the stone powder and the water-repellent agent, stirs them, and then adds other preparation raw materials during the preparation process, which can effectively improve the dispersion uniformity of the water-repellent agent in the filler and further improve the water-repellent performance of the filler. If all the raw materials are mixed and added at one time, it will have a certain impact on the water-repellent and mechanical strength of the product.

[0045] Beneficial Effects

[0046] (i) The present invention preferably mixes cement of 52.5 strength and calcium carbonate powder of 325 mesh, which can improve the strength of the sealant and reduce the cost of the product.

[0047] (ii) In order to further improve the bonding performance between the sealant and the interface to be sealed, the present invention uses ethylene-vinyl laurate-vinyl chloride copolymer terpolymer powder, which can also improve the tensile strength of the sealant and the interface bonding tensile strength.

[0048] (III) The anti-efflorescence agent of the present invention preferably has a bulk density of 350-550 g / L, a particle size of less than 250 μm, and a pH value of 8-10 (10% aqueous solution), which can significantly improve the anti-efflorescence performance of the caulking agent and improve the stability of the product.

[0049] (iv) In the present invention, sodium stearate and silicone water repellent are preferably compounded in a mass ratio of 1:(1-3) as a water repellent, which can further improve the water repellency of the sealant. At the same time, sodium stearate can form a protective film on the surface of cement particles, which can effectively prevent the aggregation of cement particles, thereby maintaining the fluidity of cement and improving the processing performance of the sealant.

[0050] (V) When preparing the single-component caulking agent of the present invention, the raw materials are added in two batches, which is conducive to the uniform dispersion of the water repellent in the system and further improves the water repellent performance of the caulking agent. DETAILED DESCRIPTION

[0051] Example 1

[0052] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.13 parts of cement, 52.16 parts of stone powder, 1.6 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.58 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0053] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0054] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0055] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0056] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0057] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0058] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0059] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0060] The mildew inhibitor is Hofmann Defros M12.

[0061] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0062] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0063] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0064] Example 2

[0065] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.31 parts of cement, 52.37 parts of stone powder, 1.21 parts of glue powder, 0.81 parts of early strength agent, 0.15 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.58 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0066] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0067] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0068] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0069] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0070] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0071] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0072] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0073] The mildew inhibitor is Hofmann Defros M12.

[0074] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0075] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0076] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0077] Example 3

[0078] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 40.12 parts of cement, 56.17 parts of stone powder, 1.6 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.58 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0079] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0080] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0081] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0082] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0083] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0084] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0085] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0086] The mildew inhibitor is Hofmann Defros M12.

[0087] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0088] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0089] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0090] Example 4

[0091] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.22 parts of cement, 52.26 parts of stone powder, 1.61 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.38 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0092] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0093] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0094] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0095] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0096] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0097] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0098] The water repellent comprises sodium stearate and Wacker powder A in a mass ratio of 1:1.

[0099] The mildew inhibitor is Hofmann Defros M12.

[0100] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0101] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0102] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0103] Comparative Example 1

[0104] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.13 parts of cement, 52.16 parts of stone powder, 1.6 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.58 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0105] The strength grade of the cement is 42.5, and the model is silver fir 52.5 grade white cement.

[0106] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0107] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0108] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0109] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0110] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0111] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0112] The mildew inhibitor is Hofmann Defros M12.

[0113] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0114] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0115] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0116] Comparative Example 2

[0117] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.30 parts of cement, 52.36 parts of stone powder, 1.61 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.19 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0118] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0119] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0120] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0121] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0122] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0123] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0124] The water repellent is sodium stearate.

[0125] The mildewcide is Hofmann Defros M12.

[0126] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0127] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0128] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0129] Comparative Example 3

[0130] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.39 parts of cement, 52.46 parts of stone powder, 1.61 parts of glue powder, 0.81 parts of early strength agent, 0.15 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, and 0.48 parts of mildew inhibitor.

[0131] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0132] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0133] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0134] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0135] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0136] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0137] The mildewcide is Hofmann Defros M12.

[0138] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0139] S1, stir the stone powder for 10 minutes;

[0140] S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30 minutes.

[0141] Comparative Example 4

[0142] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.18 parts of cement, 52.21 parts of stone powder, 1.61 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.88 parts of water repellent, and 0.48 parts of mildew inhibitor.

[0143] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0144] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0145] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0146] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0147] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0148] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0149] The mildew inhibitor is Hofmann Defros M12.

[0150] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0151] S1. Mix the stone powder and water repellent and stir for 10 minutes;

[0152] S2. Add cement, rubber powder, early strength agent, cellulose ether and mildew inhibitor, mix and stir for 30 minutes.

[0153] Comparative Example 5

[0154] The first aspect of this example provides a one-component caulking agent, the raw materials of which are calculated by weight as follows: 44.13 parts of cement, 52.16 parts of stone powder, 1.6 parts of glue powder, 0.8 parts of early strength agent, 0.14 parts of cellulose ether, 0.1 parts of anti-efflorescence agent, 0.58 parts of water repellent agent, and 0.48 parts of mildew inhibitor.

[0155] The strength grade of the cement is 52.5, and the model is silver fir 52.5 grade white cement.

[0156] The stone powder is Feiteng 325 mesh calcium carbonate white stone powder.

[0157] The early strength agent is calcium formate, purchased from Shandong Fenlian Chemical.

[0158] The rubber powder is ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder, and its model is Wacker 8034H.

[0159] The cellulose ether is hydroxyethyl methyl cellulose ether, and its model is Dow Chemical MKX 15000PP20.

[0160] The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, a pH value of 8-10, and a model of Celanese ERA-200.

[0161] The water repellent comprises sodium stearate and Wacker powder A, with a mass ratio of 19:39.

[0162] The mildew inhibitor is Hofmann Defros M12.

[0163] A second aspect of the present invention provides a method for preparing a one-component caulking agent, comprising the following steps:

[0164] S1. Mix stone powder, water repellent, cement, rubber powder, early strength agent, cellulose ether, mildew preventer and anti-efflorescence agent and stir for 40 minutes.

[0165] Performance Evaluation

[0166] 1. Basic performance test of caulking agent

[0167] Test objects: Examples 1-4, test results are shown in Table 1; test methods refer to JC / T 1004-2017.

[0168] Table 1

[0169]

[0170]

[0171] 2. Test of factors affecting cement strength

[0172] Test objects: Example 1, Comparative Example 1, test results are shown in Table 2; test method refers to JC / T1004-2017.

[0173] Table 2

[0174]

[0175]

[0176] 3. Test of factors affecting water repellent

[0177] Test objects: Example 1, Comparative Examples 2-3, test results are shown in Table 3; test method refers to JC / T1004-2017.

[0178] Table 3

[0179]

[0180] IV. Test of factors affecting anti-efflorescence agent

[0181] Test objects: Example 1, Comparative Example 4. The test results are shown in Table 4.

[0182] Table 4

[0183] Test items Example 1 Comparative Example 4 Anti-alkali No alkali return, no powder loss Slightly alkali

[0184] 5. Test of factors affecting the order of adding materials

[0185] Test objects: Example 1, Comparative Example 5, test results are shown in Table 5; test method refers to JC / T1004-2017.

[0186] Table 5

[0187] Test items Standard value Example 1 Comparative Example 5 Water absorption (30min) / g ≤2 0.9 1.2 Water absorption (240min) / g ≤5 1.8 2

Claims

1. A one-component caulking agent, characterized in that: The raw materials include cement, stone powder, rubber powder, early strength agent, cellulose ether, anti-efflorescence agent, water repellent agent and mildew preventer.

2. The one-component caulking agent according to claim 1, characterized in that: The raw materials for preparation include, by weight: 40-50 parts of cement, 50-60 parts of stone powder, 1-3 parts of rubber powder, 0.1-1 parts of early strength agent, 0.1-1 parts of cellulose ether, 0.1-1 parts of anti-efflorescence agent, 0.1-1 parts of water repellent agent, and 0.1-1 parts of mildew preventer.

3. The one-component caulking agent according to claim 1, characterized in that: The cement grade strength is 40-65.

4. The one-component caulking agent according to claim 1, characterized in that: The rubber powder comprises one of vinyl acetate-ethylene copolymer rubber powder, acrylate-styrene copolymer rubber powder, ethylene-vinyl laurate-vinyl chloride copolymer terpolymer rubber powder and styrene-butadiene copolymer rubber powder.

5. The one-component caulking agent according to claim 1, characterized in that: The early strength agent includes one of calcium chloride, sodium sulfate, gypsum, water glass, sodium aluminate, sodium carbonate, calcium carbonate, calcium formate, sodium fluoride and triethanolamine.

6. The one-component caulking agent according to claim 1, characterized in that: The cellulose ether includes: one of anionic cellulose ether, cationic cellulose ether and nonionic ether cellulose ether.

7. The one-component caulking agent according to claim 6, characterized in that: The nonionic ether cellulose ether includes: one of methyl cellulose ether, hydroxypropyl methyl cellulose ether, hydroxyethyl methyl cellulose ether and hydroxyethyl cellulose ether.

8. The one-component caulking agent according to claim 1, characterized in that: The anti-efflorescence agent has a bulk density of 350-550 g / L, a particle size of less than 250 μm, and a pH value of 8-10.

9. The one-component caulking agent according to claim 1, characterized in that: The water repellent includes an inorganic water repellent and / or an organic water repellent.

10. A method for preparing the one-component caulking agent according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Mix the stone powder and water repellent and stir for 10-30 minutes; S2. Add cement, rubber powder, early strength agent, cellulose ether, mildew inhibitor and anti-efflorescence agent, mix and stir for 30-60 minutes.