Preparation method of high-performance micro-nano cementing material

By using an intelligent control system and a specific material combination preparation method, the efficient and automated production of micro-nano cementitious materials has been achieved, solving the problems of poor corrosion resistance and high resource consumption of traditional cementitious materials, and producing high-performance, multifunctional micro-nano cementitious materials.

CN118930209APending Publication Date: 2024-11-12HAINAN JINHUAN BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002271.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional cementitious materials consume a large amount of non-renewable resources and energy during the production process, and have poor corrosion resistance and are easily affected by environmental factors, resulting in poor durability.

Method used

The entire production process is controlled by an intelligent control system. Micro-nano cementitious materials are prepared through grinding, mixing and high-temperature reaction modules. The combination of micro-nano materials, surfactants and cementitious materials, including montmorillonite, nano SiC, nano Si3N4, gypsum, lime and resin, is used to achieve automated closed production, reducing manual operation and energy consumption.

Benefits of technology

The production of micro-nano cementitious materials with finer particle size and more uniform distribution has resulted in high corrosion resistance, chloride ion penetration resistance, and water resistance, improving the durability of the materials and solving the problem of poor corrosion resistance in traditional cementitious materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930209A_ABST
    Figure CN118930209A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-performance micro-nano cementitious material, and belongs to the technical field of cementitious material preparation, and the micro-nano cementitious material comprises a micro-nano material, a surfactant and a cementitious material; the concrete comprises the following components in parts by weight: 20-30 parts of a micro-nano material, 5-10 parts of a surfactant and 60-75 parts of a cementing material, according to the preparation method of the micro-nano cementing material, an intelligent control system is adopted to implement and control the whole production process, and the intelligent control system comprises a production module, an execution module and a storage module; the whole production process is implemented and controlled by adopting an intelligent control system, and the whole production process of the micro-nano cementing material is accurately monitored, so that the produced particles of the micro-nano cementing material can achieve ideal performance, and the micro-nano cementing material composite particle powder which is stable and reliable in performance, high in performance and multifunctional is manufactured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a micro-nano gelling material, in particular to a method for preparing a high-performance micro-nano gelling material, and belongs to the technical field of gelling material preparation. Background Art

[0002] Concrete is one of the most widely used structural engineering materials in the construction field today, and plays a key role in the construction and development of my country's infrastructure. In construction engineering, any material that can transform from a slurry into a hard stone-like body and cement loose mineral materials into a whole through its own physical and chemical effects is collectively referred to as a cementitious material. As a research field at the forefront of science and technology, micro-nano materials refer to composite materials or single materials with sizes ranging from microns (1um = 10^-6m) to nanometers (1nm = 10^-9m). Applying micro-nano material technology to cementitious material technology and combining them with each other can produce a new type of micro-nano cementitious material.

[0003] However, at present, traditional cementitious materials consume a large amount of non-renewable resources and energy in the production process to prepare qualified raw materials and calcine qualified clinker. The traditional production process requires a large number of people to participate in the production, which is easy to cause dust occupational disease injuries to personnel during the production process and generate high labor costs. Moreover, since cementitious materials are easily affected by the environment during use, especially by environmental factors such as high and low temperatures, humidity and other factors, they are prone to corrosion problems, making the materials not durable and having poor durability. It is urgent to develop a high-performance new material that can make up for the shortcomings of existing materials, replace traditional production technology, and solve the problem of poor corrosion resistance of cementitious materials in the existing technology. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a high-performance micro-nano gelling material, so as to solve the problem of poor corrosion resistance of the gelling material in the prior art.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0006] A method for preparing a high-performance micro-nano gelling material, wherein the micro-nano gelling material comprises a micro-nano material, a surfactant and a gelling material; the weight parts of the components are 20-30 parts of the micro-nano material, 5-10 parts of the surfactant and 60-75 parts of the gelling material;

[0007] The preparation method of the micro-nano gelling material adopts an intelligent control system to implement and control the whole production process. The intelligent control system includes a production module, an execution module and a storage module, and includes the following steps:

[0008] S1. Constructing a production module in the intelligent control system, which is used to classify and construct the production module according to the production operation behavior and production equipment structure to be produced;

[0009] S2. Select the production module, which is used to perform production operations according to the system variables and control variables of the production module, and work in conjunction with the execution module, starting from the initial state, and sequentially executing the operations of the production module until the entire production operation is completed;

[0010] S3. After the production module operation is completed, the entire process of production data and production process parameter control is loaded into the storage module for analysis and archiving.

[0011] Furthermore, the production module includes a grinding processing module, a high temperature reaction module, a material mixing module, and a particle size detection module; the following steps are performed in sequence:

[0012] S21. Start the grinding process module, control the grinding production process according to the process parameters in the grinding process module, complete the grinding operation, and make the material particle size into powder of the desired particle size, including micro-nano material powder and gelling material powder;

[0013] S22. Start the high temperature reaction module, control the powder processing according to the process parameters in the high temperature reaction module, complete the high temperature reaction operation, and prepare the powder raw material into powder clinker, including cementitious material powder clinker;

[0014] S23. Start the material mixing module, complete the mixing operation according to the process parameter control in the material mixing module, mix the micro-nano material powder, the gelling material powder and the surfactant sufficiently and evenly, and prepare the micro-nano gelling material composite particle powder after drying;

[0015] S24. Start the particle size detection module, and complete the particle size detection of the micro-nano gelling material composite particle powder according to the process parameter control in the particle size detection module. If the particle size is qualified, it is a micro-nano gelling material. Otherwise, repeat S21 until the powder particle size is qualified.

[0016] Furthermore, the micro-nano materials are two of montmorillonite, nano-SiC, and nano-Si3N4.

[0017] Furthermore, the micro-nano material is a mixture of nano-SiC and nano-Si3N4.

[0018] Furthermore, the surfactant is one of polysiloxane phosphate salt or potassium lauryl aldehyde phosphate.

[0019] Furthermore, the cementitious material includes gypsum, lime, and resin.

[0020] Further, the weight ratio of gypsum:lime:resin is 3:3:1.

[0021] Furthermore, the resin is one of silicone resin or epoxy resin.

[0022] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:

[0023] The method of the present invention uses an intelligent control system to implement and control the entire production process, implements production technology through production modules, uses an intelligent control system to control operation, and accurately monitors the entire production process of micro-nano gelling materials, so that the particles of the produced micro-nano gelling materials can achieve ideal performance, and produce micro-nano gelling material composite particle powders with stable and reliable performance, high performance and multifunctionality. The corrosion resistance of micro-nano gelling materials is improved, and new process technology is used to replace traditional production process technology, solving the problem of poor corrosion resistance of gelling materials in the prior art.

[0024] Specifically, the powder produced has finer particle size, more uniform distribution, better dispersibility, and in addition to all the superior properties of a single particle, it also has multiple composite and synergistic functions, ensuring the high performance of micro-nano gelling materials. By combining multiple material components to enhance the performance of the material, a high-performance micro-nano gelling material is produced with high corrosion resistance, resistance to chloride ion penetration, and water resistance. The durability of the new material is enhanced and its durability is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The invention discloses a control flow chart of an intelligent control system module used in a method for preparing a micro-nano gelling material. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention and the related drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The invention discloses a method for preparing a high-performance micro-nano gelling material. The micro-nano gelling material comprises micro-nano material, surfactant and gelling material. The weight proportions of the micro-nano material are 20-30 parts, the surfactant is 5-10 parts and the gelling material is 60-75 parts.

[0028] The micro-nano materials are two of montmorillonite, nano-SiC and nano-Si3N4.

[0029] The surfactant is one of polysiloxane phosphate salt or potassium lauryl aldehyde phosphate (MAEPK).

[0030] The cementitious material includes gypsum, lime and resin; the weight ratio thereof is 3:3:1.

[0031] The resin is one of silicone resin or epoxy resin.

[0032] Micro-nano gelling material is a new type of physically modified gelling material. It is a new type of high-performance micro-nano gelling material that is compounded with micro-nano material and gelling material.

[0033] The preparation method of micro-nano gelling material adopts intelligent control system to implement and control the whole production process. For easy understanding, please refer to Figure 1 , the intelligent control system includes a production module, an execution module and a storage module, including the following steps:

[0034] S1. Constructing a production module in the intelligent control system, which is used to classify and construct the production module according to the production operation behavior and production equipment structure to be produced;

[0035] S2. Select the production module, which is used to perform production operations according to the system variables and control variables of the production module, and work in conjunction with the execution module, starting from the initial state, and sequentially executing the operations of the production module until the entire production operation is completed;

[0036] The production module includes a grinding processing module, a high temperature reaction module, a material mixing module, and a particle size detection module; the following steps are performed in sequence:

[0037] S21. Start the grinding process module, control the grinding production process according to the process parameters in the grinding process module, complete the grinding operation, and make the material particle size into powder of the desired particle size, including micro-nano material powder and gelling material powder;

[0038] S22. Start the high temperature reaction module, control the powder processing according to the process parameters in the high temperature reaction module, complete the high temperature reaction operation, and prepare the powder raw material into powder clinker, including cementitious material powder clinker;

[0039] S23. Start the material mixing module, complete the mixing operation according to the process parameter control in the material mixing module, mix the micro-nano material powder, the gelling material powder and the surfactant sufficiently and evenly, and prepare the micro-nano gelling material composite particle powder after drying;

[0040] S24. Start the particle size detection module, and complete the particle size detection of the micro-nano gelling material composite particle powder according to the process parameter control in the particle size detection module. If the particle size is qualified, it is a micro-nano gelling material. Otherwise, repeat S21 until the powder particle size is qualified;

[0041] The process parameter controls in each module in the above steps S21, S22, S23, and S24 can be adjusted according to actual production operations and are not limited here.

[0042] S3. After the production module operation is completed, the entire process of production data and production process parameter control is loaded into the storage module for analysis and archiving.

[0043] The method of the present invention adopts an intelligent control system to implement and control the entire production process, implements production technology through production modules, uses an intelligent control system to control operation, and accurately monitors the entire production process of micro-nano gelling materials, so that the particles of the produced micro-nano gelling materials can achieve ideal performance, and produce micro-nano gelling material composite particle powders with stable and reliable performance, high performance and multifunctions.

[0044] The new process technology is used to replace the traditional production process technology. The powder produced has finer particle size, more uniform distribution, and better dispersibility. In addition to the superior performance of single particles, it also has multiple composite and synergistic functions, ensuring the high performance of micro-nano gelling materials. The purpose of enhancing the performance of materials by combining multiple material components is to produce high-performance micro-nano gelling materials with high corrosion resistance, resistance to chloride ion penetration, and water resistance. The corrosion resistance of micro-nano gelling materials is improved as a whole, solving the problem of poor corrosion resistance of gelling materials in the prior art. It promotes the enhancement of the durability of materials and improves their durability.

[0045] The characteristics of using new process technology to replace traditional production process technology are as follows:

[0046] (1) The intelligent control system replaces the traditional manual production operation of the equipment. After the entire production process is started, the operation and control of different modules can be automatically carried out. There is no need for manual operation and regulation of the equipment, which reduces human operation errors and labor costs and realizes modern production.

[0047] (2) The production module replaces the traditional open production operation, realizing the fully enclosed assembly line automated production of the equipment. The production process is dust-free, avoiding dust drift and manual intervention in the production process. Therefore, it also avoids the hazards of dust occupational diseases in the production process, ensuring the health of personnel and keeping the entire production process clean and tidy.

[0048] (3) The high-temperature reaction module replaces the process operation of traditional fuel calcination production. The high-temperature reaction process does not produce calcination. All high-temperature reactions are produced using electrical energy, which reduces energy consumption and eliminates the emission of exhaust gas and other waste gases, which is beneficial to environmental protection.

[0049] Example 1

[0050] The micro-nano gelling material comprises micro-nano materials, surfactants and gelling materials;

[0051] The micro-nano material is a mixture of nano-SiC and nano-Si3N4, and the weight ratio of nano-SiC: nano-Si3N4 is 1:1;

[0052] The surfactant is polysiloxane phosphate salt;

[0053] The cementitious material includes gypsum, lime and resin; the weight ratio is 3:3:1;

[0054] The resin is a silicone resin;

[0055] Table 1: Material usage table of Example 1

[0056]

[0057] The total amount of ingredients is 1 kg, including 26 parts of micro-nano materials, 8 parts of surfactants and 66 parts of gelling materials.

[0058] The preparation method of the micro-nano gelling material adopts an intelligent control system to implement and control the whole production process. The intelligent control system includes a production module, an execution module and a storage module, and includes the following steps:

[0059] S1. Constructing a production module in the intelligent control system, which is used to classify and construct the production module according to the production operation behavior and production equipment structure to be produced;

[0060] S2. Select the production module, which is used to perform production operations according to the system variables and control variables of the production module, and work in conjunction with the execution module, starting from the initial state, and sequentially executing the operations of the production module until the entire production operation is completed;

[0061] The production module includes a grinding processing module, a high temperature reaction module, a material mixing module, and a particle size detection module; the following steps are performed in sequence:

[0062] S21. Start the grinding process module, control the grinding production process according to the process parameters in the grinding process module, complete the grinding operation, and make the material particle size into powder of the desired particle size, including micro-nano material powder and gelling material powder;

[0063] S22. Start the high temperature reaction module, control the powder processing according to the process parameters in the high temperature reaction module, complete the high temperature reaction operation, and prepare the powder raw material into powder clinker, including cementitious material powder clinker;

[0064] S23. Start the material mixing module, complete the mixing operation according to the process parameter control in the material mixing module, mix the micro-nano material powder, the gelling material powder and the surfactant sufficiently and evenly, and prepare the micro-nano gelling material composite particle powder after drying;

[0065] S24. Start the particle size detection module, and complete the particle size detection of the micro-nano gelling material composite particle powder according to the process parameter control in the particle size detection module. If the particle size is qualified, it is a micro-nano gelling material. Otherwise, repeat S21 until the powder particle size is qualified;

[0066] S3. After the production module operation is completed, the entire process of production data and production process parameter control is loaded into the storage module for analysis and archiving.

[0067] Example 2

[0068] The micro-nano gelling material comprises micro-nano materials, surfactants and gelling materials;

[0069] The micro-nano material is a mixture of nano-SiC and montmorillonite;

[0070] The weight ratio of nano-SiC:montmorillonite is 1:1;

[0071] The surfactant was potassium lauryl aldehyde phosphate (MAEPK);

[0072] The cementitious material includes gypsum, lime and resin; the weight ratio is 3:3:1;

[0073] The resin is a silicone resin;

[0074] Table 2: Material usage table of Example 2

[0075]

[0076] The total amount of ingredients is 1 kg, including 20 parts of micro-nano materials, 5 parts of surfactants and 75 parts of gelling materials.

[0077] The preparation method of the micro-nano gelling material is the same as that of Example 1.

[0078] Example 3

[0079] The micro-nano gelling material comprises micro-nano materials, surfactants and gelling materials;

[0080] The micro-nano material is a mixture of montmorillonite and nano-Si3N4;

[0081] The weight ratio of montmorillonite: nano-Si3N4 is 1:1;

[0082] The surfactant was potassium lauryl aldehyde phosphate (MAEPK);

[0083] The cementitious material includes gypsum, lime and resin; the weight ratio is 3:3:1;

[0084] The resin is epoxy resin;

[0085] Table 3: Material usage table of Example 3

[0086]

[0087] The total amount of ingredients is 1 kg, including 30 parts of micro-nano materials, 10 parts of surfactants and 60 parts of gelling materials.

[0088] The preparation method of the micro-nano gelling material is the same as that of Example 1.

[0089] Comparative Example 1

[0090] Comparative Example 1 is a comparative experiment of Example 1, except that the gelling material component does not contain a resin component, and other types of materials used, preparation methods, and process parameters are the same.

[0091] The micro-nano gelling material comprises micro-nano materials, surfactants and gelling materials;

[0092] The micro-nano material is a mixture of nano-SiC and nano-Si3N4;

[0093] The weight ratio of nano-SiC: nano-Si3N4 is 1:1;

[0094] The surfactant was potassium lauryl aldehyde phosphate (MAEPK);

[0095] The cementitious material includes gypsum and lime; the weight ratio thereof is 1:1;

[0096] Table 4: Material usage table of comparative example 1

[0097]

[0098] The total amount of ingredients is 1 kg, including 26 parts of micro-nano materials, 8 parts of surfactants and 66 parts of gelling materials.

[0099] The preparation method of the micro-nano gelling material is the same as that of Example 1.

[0100] Comparative Example 2

[0101] Comparative Example 2 is a comparative experiment of Example 1, except that the micro-nano gelling material does not include a surfactant, and other types of materials used, preparation methods, and process parameters are the same.

[0102] Micro-nano gelling materials include micro-nano materials and gelling materials;

[0103] The micro-nano material is a mixture of nano-SiC and nano-Si3N4;

[0104] The weight ratio of nano-SiC: nano-Si3N4 is 1:1;

[0105] No surfactant;

[0106] The cementitious materials include gypsum, lime and resin; the weight ratio is 3:3:1

[0107] The resin is a silicone resin;

[0108] Table 5: Material usage table of comparative example 2

[0109]

[0110] The total amount of ingredients is 1 kg, including 30 parts of micro-nano materials and 70 parts of gelling materials.

[0111] The preparation method of the micro-nano gelling material is the same as that of Example 1.

[0112] Comparative Example 3

[0113] Comparative Example 3 is a comparative experiment of Example 1, except that the micro-nano gelling material does not include micro-nano materials, and other types of materials used, preparation methods, and process parameters are the same.

[0114] The micro-nano gelling material includes a surfactant and a gelling material;

[0115] The surfactant is polysiloxane phosphate salt;

[0116] The cementitious material includes gypsum, lime and resin; the weight ratio is 3:3:1;

[0117] The resin is a silicone resin;

[0118] Table 6: Material usage table of comparative example 3

[0119]

[0120] The total amount of ingredients is 1 kg, including 20 parts of surfactant and 80 parts of gelling material.

[0121] The preparation method of the micro-nano gelling material is the same as that of Example 1.

[0122] 1. Corrosion resistance test

[0123] The material is processed into test blocks of size 100mm×100mm×100mm, 3 blocks in each group. Carefully check with a magnifying glass before the experiment, and only those without cracks can be used.

[0124] Wash the test block with clean water, dry it, and cool it naturally. Immerse the test block in a covered container filled with corrosive medium. The bottom of the test block should be elevated, the sides should be separated, and the medium liquid level should be higher than the surface of the test block. During the immersion period, the concentration of the corrosive medium should be maintained. After immersion for 45 days, take out the test block, rinse it with water, and wipe it dry with gauze.

[0125] Check the test block for cracks, peeling, expansion, corner loss, etc., and observe the discoloration of the immersion medium. If the test block is intact and there is no obvious change in the surface of the test block and the immersion medium, it is considered to be qualified in appearance and corrosion-resistant; otherwise, it is unqualified and not corrosion-resistant.

[0126] Table 7: Corrosion resistance test results

[0127] Test block type Appearance after corrosion Corrosion resistance grade Example 1 qualified Corrosion resistance Example 2 qualified Corrosion resistance Example 3 qualified Corrosion resistance Comparative Example 1 Failure Not corrosion resistant

[0128] Conclusion: By detecting the corrosion degree of different test blocks under the same conditions, it can be seen that the micro-nano gelling materials of Examples 1, 2, and 3 are relatively corrosion-resistant and have high corrosion resistance.

[0129] Compared with the comparative example 1, the micro-nano gelling material prepared is not corrosion-resistant and has low corrosion resistance. The main reason lies in the components of the gelling material. The gelling material component of comparative example 1 does not contain resin, resulting in the prepared micro-nano gelling material having low corrosion resistance, being not corrosion-resistant during use, being easily corroded by the environment such as air and humidity, and being not durable. However, in the embodiment of the present invention, by adding resin to the gelling material component and combining the resin with other component materials, the matrix material is changed, and the prepared micro-nano gelling material improves the interface bonding performance of the material after curing, is not easily corroded by the environment such as air and humidity, and is relatively durable. Therefore, the prepared micro-nano gelling material has improved corrosion resistance after curing.

[0130] 2. Chloride ion penetration resistance test

[0131] The chloride ion permeability test was carried out according to ASTM C1202-97, and the test age was 28 days.

[0132] The specific method of the experiment is as follows: a test block of size 100mm×100mm×100mm is prepared. The solutions used in the water tanks at both ends are 3.0% NaCl and 0.3N NaOH respectively. Under an external electric field of 60V, after continuous power supply for 6 hours, the total amount of electricity passing through the test block is measured. The amount of electricity passing through the test block is used to judge the test block's ability to resist chloride ion penetration.

[0133] According to the total conductivity of the concrete in 6 hours, the test block is divided into different levels of chloride ion permeability according to the conductivity. The chloride ion permeability can be judged according to the conductivity of the test block.

[0134] Table 8: Chloride ion permeability evaluation criteria

[0135] Total conductivity for 6h (Coulomb) Chloride ion permeability >4000 high 2000-4000 middle 1000-2000 Low 100-1000 Very low <100 Can be ignored

[0136] Table 9: Test results of chloride ion penetration resistance

[0137] Test block type Chloride ion permeability Example 1 Can be ignored Example 2 Very low Example 3 Can be ignored Comparative Example 2 middle

[0138] Conclusion: By testing the chloride ion permeability of different test blocks under the same conditions, it can be seen that the chloride ion permeability of the micro-nano gelling materials of Examples 1, 2, and 3 is extremely low, indicating that the chloride ion penetration resistance is relatively good.

[0139] Compared with the micro-nano gelling material prepared in Comparative Example 2, the chloride ion permeability of the prepared micro-nano gelling material is medium, the electrical conductivity is high, and the resistance to chloride ion penetration is poor. The main reason is that the components of the micro-nano gelling material do not contain surfactants, and the resistance to chloride ion penetration of the micro-nano gelling material is improved by surfactants. In the embodiment of the present invention, surfactants are added to the components of the micro-nano gelling material and formulated in proportion by weight, so that the components of the micro-nano gelling material are fully integrated with each other and have no reaction to chloride ions. The chloride ion permeability of the prepared micro-nano gelling material after solidification is extremely low, even negligible, indicating that the resistance to chloride ion penetration is good.

[0140] During use, the addition of surfactants prevents the components from reacting with chloride ions. Therefore, seawater can be used for mixing and stirring, and the product also has extremely high resistance to chloride ion penetration.

[0141] 3. Water resistance test

[0142] Water resistance is impermeability. The impermeability test experiment: refer to the specification requirements of GB / T50082-2009 for the impermeability test. This time, the penetration grade method is used to test the water resistance of the micro-nano gelling material after hardening, that is, the waterproof and impermeability performance.

[0143] Test block preparation: Each test piece is 100mm×100mm×100mm in size and is formed by manual tamping using a mold. The curing time is 28d and the mold is removed after the curing is completed.

[0144] Experimental test: Take each test block, wipe the surface, and put it into the anti-seepage instrument for testing. During the test, the water pressure starts from 0.2Mpa, and increases by 0.1Mpa every hour, and pay attention to the water seepage on the surface of the test block at any time. Keep increasing the water pressure until water seepage is found on the surface of the test block, record the water pressure at this time, and stop the test.

[0145] Table 10: Water resistance test results

[0146] Test block type Initial pressure / Mpa Water pressure resistance / Mpa Water seepage pressure / Mpa Loading time / h Example 1 0.2 1.5 1.7 15 Example 2 0.2 1.3 1.6 14 Example 3 0.2 1.3 1.5 13 Comparative Example 3 0.2 0.9 1.1 9

[0147] Conclusion: By testing the water resistance of different test blocks under the same conditions, i.e., waterproof and anti-seepage performance, it can be seen that the water resistance pressure and water seepage pressure of Examples 1, 2, and 3 are relatively high, indicating that the waterproof and anti-seepage performances are both good, i.e., high water resistance. Among them, the anti-seepage performance result of Example 1 is the best, indicating that the micro-nano gelling material prepared in Example 1 has the best water resistance.

[0148] Compared with the micro-nano gelling material prepared in Comparative Example 3, the waterproof and impermeability performance of the prepared micro-nano gelling material is poor, that is, the water resistance is low. The main reason is that the composite particle powder formed by the combination of micro-nano materials: montmorillonite, nano-SiC, and nano-Si3N4 makes the combination of the composite particle powders of each component material more compact and delicate. Specifically, the average lamella thickness of montmorillonite is less than 25nm, and it is combined with nano-SiC or nano-Si3N4 to be added to the surfactant and gelling material to prepare the micro-nano gelling material. The composite particle powder formed by the micro-nano material and the different particle powders between the components (surfactant, gelling material composite particle powder) are combined with each other, so that the pores between the composite particle powders of each component become smaller, and the smaller the pores, the higher the strength and the better the impermeability. Moreover, the addition of nano-Si3N4 also accelerates the densification speed between the composite particle powders, increases the degree of densification, and makes the powder particles more compact. Among them, the mutual composite of nano-SiC and nano-Si3N4 also greatly improves the wear resistance of the surface of the micro-nano gelling material after curing, which is reflected in the fact that the micro-nano gelling material prepared in Example 1 has high-performance composite and synergistic functions such as corrosion resistance, resistance to chloride ion penetration and water resistance.

[0149] In summary, the present invention uses an intelligent control system to implement and control the entire production process, implements production technology through a production module, uses an intelligent control system to control operation, and accurately monitors the entire production process of micro-nano gelling materials, so that the particles of the produced micro-nano gelling materials can achieve ideal performance. Produce a micro-nano gelling material composite particle powder with stable and reliable performance, high performance and multi-function. The produced powder has a finer particle size, a more uniform distribution, and better dispersibility. In addition to having all the superior properties of a single particle, it also has a composite and synergistic multiple functions, ensuring the high performance of the micro-nano gelling material. The purpose of enhancing the performance of the material by combining multiple material components is to produce a high-performance micro-nano gelling material with the characteristics of high corrosion resistance, resistance to chloride ion permeability, and water resistance. The corrosion resistance of the micro-nano gelling material is improved as a whole, solving the problem of poor corrosion resistance of the gelling material in the prior art.

[0150] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and all of them belong to the protection scope of the present application.

Claims

1. A method for preparing a high-performance micro-nano gelling material, characterized in that: The micro-nano gelling material comprises a micro-nano material, a surfactant and a gelling material; the weight proportions of the micro-nano material are 20-30 parts, the surfactant is 5-10 parts, and the gelling material is 60-75 parts; The preparation method of the micro-nano gelling material adopts an intelligent control system to implement and control the whole production process. The intelligent control system includes a production module, an execution module and a storage module, and includes the following steps: S1. Constructing a production module in the intelligent control system, which is used to classify and construct the production module according to the production operation behavior and production equipment structure to be produced; S2. Select the production module, which is used to perform production operations according to the system variables and control variables of the production module, and work in conjunction with the execution module, starting from the initial state, and sequentially executing the operations of the production module until the entire production operation is completed; S3. After the production module operation is completed, the entire process of production data and production process parameter control is loaded into the storage module for analysis and archiving.

2. The method for preparing a high-performance micro-nano gelling material according to claim 1, characterized in that: The production module includes a grinding processing module, a high temperature reaction module, a material mixing module, and a particle size detection module; the following steps are performed in sequence: S21. Start the grinding process module, control the grinding production process according to the process parameters in the grinding process module, complete the grinding operation, and make the material particle size into powder of the desired particle size, including micro-nano material powder and gelling material powder; S22. Start the high temperature reaction module, control the powder processing according to the process parameters in the high temperature reaction module, complete the high temperature reaction operation, and prepare the powder raw material into powder clinker, including cementitious material powder clinker; S23. Start the material mixing module, complete the mixing operation according to the process parameter control in the material mixing module, mix the micro-nano material powder, the gelling material powder and the surfactant sufficiently and evenly, and prepare the micro-nano gelling material composite particle powder after drying; S24. Start the particle size detection module, and complete the particle size detection of the micro-nano gelling material composite particle powder according to the process parameter control in the particle size detection module. If the particle size is qualified, it is a micro-nano gelling material. Otherwise, repeat S21 until the powder particle size is qualified.

3. The method for preparing a high-performance micro-nano gelling material according to claim 1, characterized in that: The micro-nano materials are two of montmorillonite, nano-SiC and nano-Si3N4.

4. The method for preparing a high-performance micro-nano gelling material according to claim 3, characterized in that: The micro-nano material is a mixture of nano-SiC and nano-Si3N4.

5. The method for preparing a high-performance micro-nano gelling material according to claim 4, characterized in that: The weight ratio of nano-SiC: nano-Si3N4 is 1:

1.

6. The method for preparing a high-performance micro-nano gelling material according to claim 1, characterized in that: The surfactant is one of polysiloxane phosphate salt or potassium lauryl aldehyde phosphate.

7. The method for preparing a high-performance micro-nano gelling material according to claim 1, characterized in that: Cementitious materials include gypsum, lime and resin.

8. The method for preparing a high-performance micro-nano gelling material according to claim 7, characterized in that: The weight ratio of gypsum:lime:resin is 3:3:

1.

9. The method for preparing a high-performance micro-nano gelling material according to claim 7 or 8, characterized in that: The resin is one of silicone resin or epoxy resin.