Preparation method of anti-oxidation ice ceramic

The antioxidant ice-type ceramic method with specific components stirred in distilled water solves the problem of insufficient brittleness and oxidation resistance of ceramics, achieving higher strength, stability and wide applicability, and the preparation process is simple and costly Moderate.

CN118930222APending Publication Date: 2024-11-12FUJIAN XIA SHANG ZHOU ANCIENT CELADON TECHNOLOGY CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411135532.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When used as tableware and wine utensils, existing ceramics cannot be used for a long time due to their weak brittleness and antioxidant properties, and are prone to falling and damage, and the product quality is unstable and lacks permeability.

Method used

Using an antioxidant ice-type ceramic preparation method, the potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract and SiC extract in distilled water After mechanical stirring, it is fired to produce oxidative ice-resistant ceramics.

Benefits of technology

It improves the strength and oxidation resistance of the ceramic, making it more heat-resistant, beautiful and stable, has a wider range of applicable scenarios, is simple in preparation, and is moderate in raw material costs, which is suitable for promotion and use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of ceramics, in particular to a preparation method of anti-oxidation ice ceramic which comprises the following components in percentage by weight: 4-5 parts of potassium sodium sand extract, 3-4.5 parts of kaolin extract, 0.1-0.5 part of zirconium oxide, 0.1-0.5 part of bentonite, 0.5-0.7 part of Weiluo clay extract, 0.01-0.1 part of nano silicon carbide, 0.1-0.5 part of carbon fiber extract, 0.05-0.1 part of SiC extract and a proper amount of distilled water. Compared with existing ceramics, the ceramic prepared through the preparation method has the stable physical characteristics and chemical characteristics of high strength, stable oxidation resistance, attractiveness, heat resistance and the like, so that the application scene of the ceramic is wider, and in addition, the preparation method of the ceramic is simple in procedure, moderate in raw material cost and suitable for application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramics, and in particular to a method for preparing anti-oxidation ice-type ceramics. Background Art

[0002] Ceramics is an ancient and exquisite material. It is made of natural minerals such as clay and fired at high temperatures. Ceramic products have the characteristics of high hardness, corrosion resistance, and insulation. From simple and elegant pottery to exquisite porcelain, ceramics are widely used in life, such as tableware, decorations, building materials, etc., which are both practical and artistic.

[0003] The invention patent with application number 202310219270.0 discloses a method for preparing ice jade ceramic tiles, characterized in that the method comprises the following steps: (1) mixing mineral raw materials to obtain a mineral raw material mixture, and ball milling the mixture to a set fineness by a ball mill to obtain mineral powder; wherein the mineral raw material mixture comprises the following chemical components by weight: 50-80 parts of SiO2, 10-25 parts of Al2O3, 0-1.5 parts of Ca0, 0-2.5 parts of MgO, 5-13 parts of K20, 1-5 parts of Na20, and Ca0 and Mg0 are present in the mineral raw material mixture; (2) the mineral powder is slurried, iron-removed, and spray-pulverized to obtain a powder of a desired particle size, which is then aged and homogenized to obtain a digital powder; (3) the digital powder is spread and pressed into bricks through a digital powder spraying machine, and then fired to obtain an ice jade ceramic brick.

[0004] The application aims to solve the problem that "the existing technology still has problems such as unstable product quality and insufficient transparency. Therefore, it is necessary to develop an ice jade ceramic tile with high light transmittance and stable product quality."

[0005] However, when ceramics are used as tableware and wine utensils, they cannot be used for a long time due to their brittleness and weak antioxidant properties, and are easily damaged. To this end, we proposed a method for preparing antioxidant ice-type ceramics. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing anti-oxidation ice-type ceramics, which solves the technical problems raised in the above-mentioned background technology.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: In the first aspect, an antioxidant ice-type ceramic is composed of the following components by weight percentage: 4 to 5 parts of potassium sodium sand extract, 3 to 4.5 parts of kaolin extract, 0.1 to 0.5 parts of zirconium oxide, 0.1 to 0.5 parts of bentonite, 0.5 to 0.7 parts of Vero ball clay extract, 0.01 to 0.1 parts of nano silicon carbide, 0.1 to 0.5 parts of carbon fiber extract, 0.05 to 0.1 parts of SiC extract and an appropriate amount of distilled water.

[0008] Furthermore, the preparation method of the potassium sodium sand extract is: Put potassium-sodium sand of not less than the formula percentage into a crusher for crushing, set the crusher speed to 1000-1500 rpm, and the crushing time to 15-30 min; take out the crushed potassium-sodium sand from the crusher, and use a 150-200 mesh sieve to screen the crushed potassium-sodium sand; use a glass container to receive the sieved potassium-sodium sand, further perform magnetic separation and iron removal, remove the magnetized material in the sieved potassium-sodium sand, and record it as a semi-finished potassium-sodium sand; put the semi-finished potassium-sodium sand into a 1-2 mol / L dilute hydrochloric acid solution, heat it to 60-80 degrees Celsius, stir and react for 2-4 hours, take it out and dry it; put the dried semi-finished potassium-sodium sand into a 2- 3 mol / L sodium hydroxide solution, heated to 80-100 degrees Celsius and stirred for reaction for 3-5 hours, the result is recorded as hydrous potassium-sodium sand; the hydrous potassium-sodium sand is transferred to a drying oven for drying, the drying oven temperature is set at 100 degrees Celsius to 120 degrees Celsius, the result is recorded as potassium-sodium sand extract.

[0009] Furthermore, when the semi-finished potassium sodium sand is put into a 1-2 mol / L dilute hydrochloric acid solution, the ratio of the semi-finished potassium sodium to the dilute hydrochloric acid solution is 1 / 3, and when the dried semi-finished potassium sodium sand is put into a 2-3 mol / L sodium hydroxide solution, the ratio of the dried semi-finished potassium sodium sand to the sodium hydroxide solution is 1 / 2.

[0010] Furthermore, the preparation method of the kaolin extract is: Take no less than the formula percentage of kaolin and grind it with a grinder. The grinding time is set to 20-30 minutes, and the result is recorded as mineral powder; the mineral powder, distilled water and dispersant are put into a blender for mixing and stirring, and the blender speed is set to 500-1000 rpm and the stirring time is set to 10-17 minutes; the mixture obtained by stirring is dehydrated with a centrifuge and dried with a dryer so that the water content of the mixture obtained by stirring does not exceed 1%, and the result is recorded as kaolin extract.

[0011] Furthermore, after the mineral powder, distilled water and dispersant are put into a mixer and mixed, a magnetic separator is used to remove magnetic impurities in the mixture; The ratio of the mineral powder to distilled water and dispersant is: 1 / 1.2 / 0.1; The dispersant is sodium hexametaphosphate. Before the mixture is stirred and dehydrated and dried, oxalic acid is added to the mixture for bleaching. The ratio of the mixture to oxalic acid is 1 / 0.05.

[0012] Furthermore, the preparation method of the Vero clay extract is: Take not less than the formula percentage of Veroball clay, use sorting equipment to remove non-clay impurities such as stones in the Veroball clay; use drying equipment to dry the Veroball clay with impurities and stones removed to reduce the moisture content to 10%-15%; use a strong crusher to crush the dried Veroball clay to make the clay particles meet the requirements of 1-10 microns; add oxalic acid and distilled water to the crushed Veroball clay, stir and precipitate to remove metal impurities; use hot air or infrared to dry the Veroball clay with the metal impurities removed, and set the drying temperature to 40 degrees Celsius to 80 degrees Celsius. The dried product is recorded as Veroball clay extract.

[0013] Furthermore, in the drying stage of the Vero ball clay after removing impurities and stones, the drying temperature is set to 100-120 degrees Celsius, and when the Vero ball clay after removing impurities and stones is dried, the shape is flat, and the flat thickness is not more than 1 cm; When the dried Vero ball clay is crushed by a powerful crusher, the speed of the powerful crusher is set to 1500-3000 rpm and the crushing time is set to 10 min. The ratio of crushed Vero clay, oxalic acid and distilled water is 1 / 0.1 / 0.5.

[0014] Furthermore, the zirconium oxide is any one of tetragonal zirconium oxide or cubic zirconium oxide; The zirconium oxide is preferably cubic zirconium oxide.

[0015] Furthermore, the SiC extract is extracted by any one of the preparation methods selected from the group consisting of gas phase reaction method, solid material method, nano-carbon tube template method, nano-scale droplet epitaxy method, sol-gel method and carbon thermal reduction method, carbon thermal reduction method, and chemical vapor deposition method.

[0016] In a second aspect, a method for preparing an anti-oxidation ice-type ceramic comprises the following steps: Step 1: Accurately weigh each raw material according to the above formula, and save each raw material for later use; Step 2: adding potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract, and SiC extract into distilled water for mechanical stirring; Step 3: The mixture obtained in step 2 is recorded as clay; Step 4: Knead the clay into a predetermined shape and fire it to produce antioxidant ice-type ceramics.

[0017] Compared with the known public technology, the technical solution provided by the present invention has the following beneficial effects: The present invention provides a method for preparing anti-oxidation ice-type ceramics. Compared with existing ceramics, the anti-oxidation ice-type ceramics have stable physical and chemical properties such as high strength, stable anti-oxidation performance, beautiful appearance, and heat resistance, which makes it more applicable. In addition, the preparation method of the ceramics has a relatively simple process and a moderate raw material cost, and is suitable for popularization and use. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The present invention will be further described below in conjunction with the embodiments.

[0020] Embodiment 1: An antioxidant ice-type ceramic of the present embodiment is composed of the following components by weight percentage: 4 to 5 parts of potassium sodium sand extract, 3 to 4.5 parts of kaolin extract, 0.1 to 0.5 parts of zirconium oxide, 0.1 to 0.5 parts of bentonite, 0.5 to 0.7 parts of Vero ball clay extract, 0.01 to 0.1 parts of nano silicon carbide, 0.1 to 0.5 parts of carbon fiber extract, 0.05 to 0.1 parts of SiC extract and an appropriate amount of distilled water; The preparation method of potassium sodium sand extract is: Put potassium-sodium sand of not less than the formula percentage into a crusher for crushing, set the crusher speed to 1000-1500 rpm, and the crushing time to 15-30 min; take out the crushed potassium-sodium sand from the crusher, and use a 150-200 mesh sieve to screen the crushed potassium-sodium sand; use a glass container to receive the sieved potassium-sodium sand, further perform magnetic separation and iron removal, remove the magnetized material in the sieved potassium-sodium sand, and record it as a semi-finished potassium-sodium sand; put the semi-finished potassium-sodium sand into a 1-2 mol / L dilute hydrochloric acid solution, heat it to 60-80 degrees Celsius, stir and react for 2-4 hours, take it out and dry it; put the dried semi-finished potassium-sodium sand into a 2- 3 mol / L sodium hydroxide solution, heated to 80-100 degrees Celsius and stirred for reaction for 3-5 hours, the result is recorded as hydrated potassium-sodium sand; the hydrated potassium-sodium sand is transferred to a drying oven for drying, the drying oven temperature is set at 100 degrees Celsius to 120 degrees Celsius, the result is recorded as potassium-sodium sand extract; When the semi-finished potassium sodium sand is put into a 1-2 mol / L dilute hydrochloric acid solution, the ratio of the semi-finished potassium sodium to the dilute hydrochloric acid solution is 1 / 3; when the dried semi-finished potassium sodium sand is put into a 2-3 mol / L sodium hydroxide solution, the ratio of the dried semi-finished potassium sodium sand to the sodium hydroxide solution is 1 / 2; The preparation method of kaolin extract is as follows: Take no less than the formula percentage of kaolin and grind it with a grinder, set the grinding time to 20 to 30 minutes, and the result is recorded as mineral powder; put the mineral powder, distilled water and dispersant into a blender for mixing and stirring, set the blender speed to 500 to 1000 revolutions per minute, and set the stirring time to 10 to 17 minutes; dehydrate the mixture obtained by stirring with a centrifuge and dry it with a dryer, so that the water content of the mixture obtained by stirring does not exceed 1%, and the result is recorded as kaolin extract; After the mineral powder, distilled water and dispersant are put into the mixer for mixing, a magnetic separator is used to remove magnetic impurities in the mixture; The ratio of mineral powder to distilled water and dispersant is: 1 / 1.2 / 0.1; Sodium hexametaphosphate is used as the dispersant. Before the mixture is stirred and dehydrated and dried, oxalic acid is added to the mixture for bleaching. The ratio of the mixture to oxalic acid is 1 / 0.05. The preparation method of Veroball clay extract is: Take not less than the formula percentage of Veroball clay, use sorting equipment to remove non-clay impurities such as stones in the Veroball clay; use drying equipment to dry the Veroball clay with impurities and stones removed, so that the moisture content is reduced to 10%-15%; use a strong crusher to crush the dried Veroball clay so that the clay particles meet the requirements of 1-10 microns; add oxalic acid and distilled water to the crushed Veroball clay, stir and precipitate to remove metal impurities; use hot air or infrared to dry the Veroball clay with the metal impurities removed, and set the drying temperature to 40 degrees Celsius to 80 degrees Celsius. The dried product is recorded as a Veroball clay extract; In the drying stage of the Vero ball clay after removing impurities and stones, the drying temperature is set at 100-120 degrees Celsius. When the Vero ball clay after removing impurities and stones is dried, the shape is flat, and the flat thickness is not more than 1 cm; When the dried Vero ball clay is crushed by a powerful crusher, the speed of the powerful crusher is set to 1500-3000 rpm and the crushing time is set to 10 min. The ratio of crushed Vero clay, oxalic acid and distilled water is 1 / 0.1 / 0.5; Zirconia is either tetragonal zirconia or cubic zirconia; The zirconium oxide is preferably cubic zirconium oxide; The SiC extract is extracted by any one of the preparation methods of gas phase reaction method, solid material method, carbon nanotube template method, nanoscale droplet epitaxy method, sol-gel method and carbothermal reduction method, carbothermal reduction method, and chemical vapor deposition method; A method for preparing an anti-oxidation ice-type ceramic comprises the following steps: Step 1: Accurately weigh each raw material according to the above formula, and save each raw material for later use; Step 2: adding potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract, and SiC extract into distilled water for mechanical stirring; Step 3: The mixture obtained in step 2 is recorded as clay; Step 4: Knead the clay into a predetermined shape and fire it to produce antioxidant ice-type ceramics.

[0021] Embodiment 2: An antioxidant ice-type ceramic, composed of the following components by weight percentage: 4 parts of potassium sodium sand extract, 3 parts of kaolin extract, 0.1 parts of zirconium oxide, 0.1 parts of bentonite, 0.5 parts of Vero ball clay extract, 0.01 parts of nano silicon carbide, 0.1 parts of carbon fiber extract, 0.05 parts of SiC extract and appropriate amount of distilled water; The preparation method of potassium sodium sand extract is: Take potassium-sodium sand of not less than the formula percentage and put it into a crusher for crushing treatment, set the crusher speed to 1000 rpm and the crushing time to 15 minutes; take out the crushed potassium-sodium sand from the crusher, and use a 150-mesh sieve to screen the crushed potassium-sodium sand; use a glass container to receive the sieved potassium-sodium sand that has been crushed, further perform magnetic separation and iron removal treatment, remove the magnetized matter in the sieved potassium-sodium sand that has been crushed, and record it as semi-finished potassium-sodium sand; put the semi-finished potassium-sodium sand into a 1 mol / L dilute hydrochloric acid solution, heat it to 60 degrees Celsius, stir and react for 2 hours, take it out and dry it; put the dried semi-finished potassium-sodium sand into a 2 mol / L sodium hydroxide solution, heat it to 80 degrees Celsius, stir and react for 3 hours, and the result is recorded as hydrous potassium-sodium sand; transfer the hydrous potassium-sodium sand to a drying oven for drying, and the temperature of the drying oven is set to 100 degrees Celsius, and the result is recorded as potassium-sodium sand extract; When the semi-finished potassium sodium sand is put into 1 mol / L dilute hydrochloric acid solution, the ratio of the semi-finished potassium sodium to the dilute hydrochloric acid solution is 1 / 3; when the dried semi-finished potassium sodium sand is put into 2 mol / L sodium hydroxide solution, the ratio of the dried semi-finished potassium sodium sand to the sodium hydroxide solution is 1 / 2; The preparation method of kaolin extract is as follows: Take no less than the formula percentage of kaolin and grind it with a grinder, set the grinding time to 20 minutes, and the result is recorded as mineral powder; put the mineral powder, distilled water and dispersant into a blender for mixing and stirring, set the blender speed to 500 rpm, and set the stirring time to 10 minutes; dehydrate the mixture obtained by stirring with a centrifuge and dry it with a dryer, so that the water content of the mixture obtained by stirring does not exceed 1%, and the result is recorded as kaolin extract; After the mineral powder, distilled water and dispersant are put into the mixer for mixing, a magnetic separator is used to remove magnetic impurities in the mixture; The ratio of mineral powder to distilled water and dispersant is: 1 / 1.2 / 0.1; Sodium hexametaphosphate is used as the dispersant. Before the mixture is stirred and dehydrated and dried, oxalic acid is added to the mixture for bleaching. The ratio of the mixture to oxalic acid is 1 / 0.05. The preparation method of Veroball clay extract is: Take a Veroball clay of not less than the formula percentage, use a sorting device to remove non-clay impurities such as stones in the Veroball clay; use a drying device to dry the Veroball clay from which impurities and stones are removed, so that the moisture content is reduced to 10%; use a strong crusher to crush the dried Veroball clay so that the clay particles meet the requirements of 1 micron; add oxalic acid and distilled water to the crushed Veroball clay, stir and precipitate to remove metal impurities; use hot air or infrared to dry the Veroball clay from which metal impurities are removed, and the drying temperature is set to 40 degrees Celsius. The dried product is recorded as a Veroball clay extract; In the drying stage of the Vero ball clay after removing impurities and stones, the drying temperature is set to 100 degrees Celsius. When the Vero ball clay after removing impurities and stones is dried, the shape is flat, and the flat thickness is not more than 1 cm; When the dried Vero ball clay is crushed by a powerful crusher, the speed of the powerful crusher is set to 1500 rpm and the crushing time is set to 10 min. The ratio of crushed Vero clay, oxalic acid and distilled water is 1 / 0.1 / 0.5; Zirconia is either tetragonal zirconia or cubic zirconia; The zirconium oxide is preferably cubic zirconium oxide; The SiC extract is extracted by any one of the preparation methods of gas phase reaction method, solid material method, carbon nanotube template method, nanoscale droplet epitaxy method, sol-gel method and carbothermal reduction method, carbothermal reduction method, and chemical vapor deposition method; A method for preparing an anti-oxidation ice-type ceramic comprises the following steps: Step 1: Accurately weigh each raw material according to the above formula, and save each raw material for later use; Step 2: adding potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract, and SiC extract into distilled water for mechanical stirring; Step 3: The mixture obtained in step 2 is recorded as clay; Step 4: Knead the clay into a predetermined shape and fire it to produce antioxidant ice-type ceramics.

[0022] Embodiment 3: An antioxidant ice-type ceramic, composed of the following components by weight percentage: 5 parts of potassium sodium sand extract, 4.5 parts of kaolin extract, 0.5 parts of zirconium oxide, 0.5 parts of bentonite, 0.7 parts of Vero ball clay extract, 0.1 parts of nano silicon carbide, 0.5 parts of carbon fiber extract, 0.1 parts of SiC extract and appropriate amount of distilled water; The preparation method of potassium sodium sand extract is: Put potassium-sodium sand of not less than the formula percentage into a crusher for crushing, set the crusher speed to 1500 rpm and the crushing time to 30 min; take out the crushed potassium-sodium sand from the crusher, and use a 200-mesh sieve to screen the crushed potassium-sodium sand; use a glass container to receive the sieved potassium-sodium sand that has been crushed, further perform magnetic separation and iron removal, remove the magnetized material in the sieved potassium-sodium sand that has been crushed, and record it as semi-finished potassium-sodium sand; put the semi-finished potassium-sodium sand into a 2 mol / L dilute hydrochloric acid solution, heat it to 80 degrees Celsius, stir and react for 4 hours, take it out and dry it; put the dried semi-finished potassium-sodium sand into a 3 mol / L sodium hydroxide solution, heat it to 100 degrees Celsius, stir and react for 5 hours, and the result is recorded as hydrated potassium-sodium sand; transfer the hydrated potassium-sodium sand to a drying oven for drying, and the temperature of the drying oven is set to 120 degrees Celsius, and the result is recorded as potassium-sodium sand extract; When the semi-finished potassium sodium sand is put into a 2mol / L dilute hydrochloric acid solution, the ratio of the semi-finished potassium sodium to the dilute hydrochloric acid solution is 1 / 3; when the dried semi-finished potassium sodium sand is put into a 3mol / L sodium hydroxide solution, the ratio of the dried semi-finished potassium sodium sand to the sodium hydroxide solution is 1 / 2; The preparation method of kaolin extract is as follows: Take no less than the formula percentage of kaolin and grind it with a grinder, set the grinding time to 30 minutes, and the result is recorded as mineral powder; put the mineral powder, distilled water and dispersant into a blender for mixing and stirring, set the blender speed to 1000 rpm, and set the stirring time to 17 minutes; dehydrate the mixture obtained by stirring with a centrifuge and dry it with a dryer, so that the water content of the mixture obtained by stirring does not exceed 1%, and the result is recorded as kaolin extract; After the mineral powder, distilled water and dispersant are put into the mixer for mixing, a magnetic separator is used to remove magnetic impurities in the mixture; The ratio of mineral powder to distilled water and dispersant is: 1 / 1.2 / 0.1; Sodium hexametaphosphate is used as the dispersant. Before the mixture is stirred and dehydrated and dried, oxalic acid is added to the mixture for bleaching. The ratio of the mixture to oxalic acid is 1 / 0.05. The preparation method of Veroball clay extract is: Take not less than the formula percentage of Veroball clay, use sorting equipment to remove non-clay impurities such as stones in the Veroball clay; use drying equipment to dry the Veroball clay with impurities and stones removed to reduce the moisture content to 15%; use a strong crusher to crush the dried Veroball clay to make the clay particles meet the requirements of 10 microns; add oxalic acid and distilled water to the crushed Veroball clay, stir and precipitate to remove metal impurities; use hot air or infrared to dry the Veroball clay with the metal impurities removed, and set the drying temperature to 80 degrees Celsius. The dried product is recorded as a Veroball clay extract; In the drying stage of the Vero ball clay after removing impurities and stones, the drying temperature is set to 120 degrees Celsius. When the Vero ball clay after removing impurities and stones is dried, the shape is flat, and the flat thickness is not more than 1 cm; When the dried Vero ball clay is crushed by a powerful crusher, the speed of the powerful crusher is set to 3000 rpm and the crushing time is set to 10 min. The ratio of crushed Vero clay, oxalic acid and distilled water is 1 / 0.1 / 0.5; Zirconia is either tetragonal zirconia or cubic zirconia; The zirconium oxide is preferably cubic zirconium oxide; The SiC extract is extracted by any one of the preparation methods of gas phase reaction method, solid material method, carbon nanotube template method, nanoscale droplet epitaxy method, sol-gel method and carbothermal reduction method, carbothermal reduction method, and chemical vapor deposition method; A method for preparing an anti-oxidation ice-type ceramic comprises the following steps: Step 1: Accurately weigh each raw material according to the above formula, and save each raw material for later use; Step 2: adding potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract, and SiC extract into distilled water for mechanical stirring; Step 3: The mixture obtained in step 2 is recorded as clay; Step 4: Knead the clay into a predetermined shape and fire it to produce antioxidant ice-type ceramics.

[0023] In summary, the ceramics obtained by the method for preparing anti-oxidative ice ceramics in the above embodiment have stable physical and chemical properties such as high strength, stable anti-oxidative performance, beautiful appearance, and heat resistance, which makes it applicable to a wider range of scenarios. In addition, the preparation method of this type of ceramics has a relatively simple process and a moderate raw material cost, and is suitable for promotion and use.

[0024] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An anti-oxidation ice-type ceramic, characterized in that: The invention is composed of the following components by weight percentage: 4 to 5 parts of potassium sodium sand extract, 3 to 4.5 parts of kaolin extract, 0.1 to 0.5 parts of zirconium oxide, 0.1 to 0.5 parts of bentonite, 0.5 to 0.7 parts of Vero ball clay extract, 0.01 to 0.1 parts of nano silicon carbide, 0.1 to 0.5 parts of carbon fiber extract, 0.05 to 0.1 parts of SiC extract and appropriate amount of distilled water.

2. The anti-oxidation ice-type ceramic according to claim 1, characterized in that: The preparation method of the potassium sodium sand extract is: Put potassium-sodium sand of not less than the formula percentage into a crusher for crushing, set the crusher speed to 1000-1500 rpm, and the crushing time to 15-30 min; take out the crushed potassium-sodium sand from the crusher, and use a 150-200 mesh sieve to screen the crushed potassium-sodium sand; use a glass container to receive the sieved potassium-sodium sand, further perform magnetic separation and iron removal, remove the magnetized material in the sieved potassium-sodium sand, and record it as a semi-finished potassium-sodium sand; put the semi-finished potassium-sodium sand into a 1-2 mol / L dilute hydrochloric acid solution, heat it to 60-80 degrees Celsius, stir and react for 2-4 hours, take it out and dry it; put the dried semi-finished potassium-sodium sand into a 2- 3 mol / L sodium hydroxide solution, heated to 80-100 degrees Celsius and stirred for reaction for 3-5 hours, the result is recorded as hydrous potassium-sodium sand; the hydrous potassium-sodium sand is transferred to a drying oven for drying, the drying oven temperature is set at 100 degrees Celsius to 120 degrees Celsius, the result is recorded as potassium-sodium sand extract.

3. The anti-oxidation ice-type ceramic according to claim 2, characterized in that: When the semi-finished potassium sodium sand is put into 1-2mol / L dilute hydrochloric acid solution, the ratio of the semi-finished potassium sodium to the dilute hydrochloric acid solution is 1 / 3. When the dried semi-finished potassium sodium sand is put into 2-3mol / L sodium hydroxide solution, the ratio of the dried semi-finished potassium sodium sand to the sodium hydroxide solution is 1 / 2.

4. The anti-oxidation ice-type ceramic according to claim 1, characterized in that: The preparation method of the kaolin extract is: Take no less than the formula percentage of kaolin and grind it with a grinder. The grinding time is set to 20-30 minutes, and the result is recorded as mineral powder; the mineral powder, distilled water and dispersant are put into a blender for mixing and stirring, and the blender speed is set to 500-1000 rpm and the stirring time is set to 10-17 minutes; the mixture obtained by stirring is dehydrated with a centrifuge and dried with a dryer so that the water content of the mixture obtained by stirring does not exceed 1%, and the result is recorded as kaolin extract.

5. The anti-oxidation ice-type ceramic according to claim 4, characterized in that: After the mineral powder, distilled water and dispersant are put into a mixer for mixing, a magnetic separator is used to remove magnetic impurities in the mixture; The ratio of the mineral powder to distilled water and dispersant is: 1 / 1.2 / 0.1; The dispersant is sodium hexametaphosphate. Before the mixture is stirred and dehydrated and dried, oxalic acid is added to the mixture for bleaching. The ratio of the mixture to oxalic acid is 1 / 0.

05.

6. The anti-oxidation ice-type ceramic according to claim 1, characterized in that: The preparation method of the Veroball clay extract is: Take not less than the formula percentage of Veroball clay, use sorting equipment to remove non-clay impurities such as stones in the Veroball clay; use drying equipment to dry the Veroball clay with impurities and stones removed to reduce the moisture content to 10%-15%; use a strong crusher to crush the dried Veroball clay to make the clay particles meet the requirements of 1-10 microns; add oxalic acid and distilled water to the crushed Veroball clay, stir and precipitate to remove metal impurities; The Veroball clay from which metal impurities have been removed is dried using hot air or infrared, the drying temperature is set at 40 degrees Celsius to 80 degrees Celsius, and the dried extract is recorded as the Veroball clay extract.

7. The anti-oxidation ice-type ceramic according to claim 6, characterized in that: In the drying stage of the Vero ball clay after removing impurities and stones, the drying temperature is set at 100-120 degrees Celsius. When the Vero ball clay after removing impurities and stones is dried, the shape is flat, and the flat thickness is not more than 1 cm; When the dried Vero ball clay is crushed by a powerful crusher, the speed of the powerful crusher is set to 1500-3000 rpm and the crushing time is set to 10 min. The ratio of crushed Vero clay, oxalic acid and distilled water is 1 / 0.1 / 0.

5.

8. The anti-oxidation ice-type ceramic according to claim 1, characterized in that: The zirconium oxide is any one of tetragonal zirconium oxide or cubic zirconium oxide; The zirconium oxide is preferably cubic zirconium oxide.

9. The anti-oxidation ice-type ceramic according to claim 1, characterized in that: The SiC extract is extracted by any one of the following preparation methods: gas phase reaction method, solid material method, nano carbon tube template method, nanoscale droplet epitaxy method, sol-gel method and carbon thermal reduction method, carbon thermal reduction method, and chemical vapor deposition method.

10. A method for preparing an anti-oxidation ice-type ceramic, the method being a method for preparing an anti-oxidation ice-type ceramic as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Accurately weigh each raw material according to the above formula, and save each raw material for later use; Step 2: adding potassium sodium sand extract, kaolin extract, zirconium oxide, bentonite, Vero ball clay extract, nano silicon carbide, carbon fiber extract, and SiC extract into distilled water for mechanical stirring; Step 3: The mixture obtained in step 2 is recorded as clay; Step 4: Knead the clay into a predetermined shape and fire it to produce antioxidant ice-type ceramics.

Citation Information

Patent Citations

  • Alumina-zirconia-silicon carbide-magnesia ceramic cutting tools

    CA1332106C

  • Self-repairing aluminum oxide-based ceramic composite material and preparation thereof

    CN101407411A

  • Method of purification of potash feldspar and soda feldspar ores

    CN109052423A

  • Kaolin processing technology

    CN112707403A

  • High-toughness conical suspension type porcelain insulator and preparation method thereof

    CN113443892A