MgO ceramic material prepared by low-temperature sintering and preparation method thereof

By adding alumina and magnesium fluoride to magnesium oxide ceramics, forming a MgO gel liquid and sintering under low-temperature sintering conditions, the problem of high sintering temperature of magnesium oxide ceramics is solved, and high density and good thermal conductivity are achieved Preparation of ceramic materials.

CN118930229AActive Publication Date: 2024-11-12HUNAN UNIV OF TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410908162.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The high sintering temperature of magnesium oxide ceramics leads to high costs, loose structure, low strength and poor thermal conductivity, and low-temperature sintering cannot be dense.

Method used

A mixed powder with a mass ratio of magnesium oxide, alumina and magnesium fluoride of 95:5:3 to 5 was used, and then mixed with organic substances through ball milling and acidic solution to form a gelatinous liquid. After dehydration and degreasing treatment, it is used. Sintering at 1400-1450°C, the melting point is reduced by MgF2 and the solid solution of Al2O3 are improved.

Benefits of technology

Low-temperature sintering is achieved to prepare MgO ceramics, which have excellent mechanical properties and good thermal conductivity, and greatly reduce the firing temperature to obtain ceramic materials with a density of more than 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930229A_ABST
    Figure CN118930229A_ABST
Patent Text Reader

Abstract

The invention discloses an MgO ceramic material prepared through low-temperature sintering and a preparation method thereof. According to the MgO ceramic material prepared through low-temperature sintering and the preparation method thereof, aluminum oxide and magnesium fluoride are added into magnesium oxide ceramic, the sintering temperature of a mixture can be reduced through MgF2, the porosity number and size can be reduced through Al2O3, the density of MgO is improved, the temperature of the MgO ceramic is reduced, and the MgO ceramic can be compact at the low temperature. MgO powder is mixed with a monomer, a cross-linking agent, a dispersing agent and the like, so that MgO gel-state liquid is homogenized, agglomeration of magnesium oxide is avoided, the method is lower in sintering temperature, energy consumption is reduced, the experimental period is shortened, the density of MgO ceramic is 90% or above, and the MgO ceramic has excellent mechanical properties and good heat conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnesium oxide thermal conductive ceramics, and more specifically, relates to a MgO ceramic material prepared by low-temperature sintering and a preparation method thereof. Background Art

[0002] Magnesium oxide ceramics are widely used in high-tech, high-precision and advanced fields due to their excellent properties such as high strength, corrosion resistance and wear resistance. However, the production of high-quality magnesium oxide ceramics has the following difficulties:

[0003] (1) During the production process, magnesium oxide powder easily absorbs moisture in the air and agglomerates, which affects the fluidity of the powder and makes it difficult to disperse the powder evenly.

[0004] (2) Magnesium oxide ceramics need to be sintered at a temperature above 1700°C, which is not only costly but also difficult to control the crystal phase. The resulting green body has a loose structure, low strength, and poor thermal conductivity.

[0005] In order to solve the above problems, CN104276815B discloses an oxide ceramic material and a preparation method thereof. The raw material components include 70% to 96% magnesium oxide, 2% to 25% aluminum oxide, 0.2% to 1.2% silicon dioxide, 0.2% to 2.5% calcium oxide, 0.1% to 0.5% iron oxide and 0.5% to 1.5% zircon. Through ball milling, waxing, molding, initial firing, body trimming, firing and post-processing, a new type of high thermal conductivity ceramic material with high density and low cost and a sintering temperature of only 1650°C is obtained. This patent uses the fact that when magnesium oxide and aluminum oxide transform from tetragonal phase to cubic phase, zirconium oxide can expand first and then contract during the phase change process, adapting to the volume change of the phase change process between other materials, so that the dislocation and porosity of the crystals are reduced, the damage tolerance of the material preparation during sintering is enhanced, the diffusion of cracks is inhibited or prevented, and the density and fracture toughness of magnesium oxide ceramics are increased. Silicon dioxide and calcium oxide are used to reduce the sintering temperature, and the product has high acid resistance and can improve the product's resistance to acid corrosion. Although this method reduces the sintering temperature through silicon dioxide and calcium oxide, its sintering temperature still needs to be above 1600°C. If this sintering temperature cannot be reached, magnesium oxide ceramics cannot maintain a high density. Summary of the invention

[0006] The present invention provides a MgO ceramic material prepared by low-temperature sintering and a preparation method thereof in order to overcome the problem that the existing MgO ceramic has a high sintering temperature and cannot be dense by low-temperature sintering.

[0007] The present invention is achieved through the following technical solutions:

[0008] A MgO ceramic material prepared by low-temperature sintering, the raw materials of which include magnesium oxide, aluminum oxide and magnesium fluoride, wherein the mass ratio of the magnesium oxide, aluminum oxide and magnesium fluoride is 95:5:3-5.

[0009] A method for preparing a MgO ceramic material prepared by low temperature sintering, the preparation steps comprising:

[0010] S1. The magnesium oxide, aluminum oxide and magnesium fluoride powders are mixed uniformly in a mass ratio to obtain a mixed powder;

[0011] S2. The mixed powder is mixed with an organic matter to obtain a mixed slurry, and then the mixed slurry is vacuum treated to obtain a MgO gel liquid;

[0012] S3. The MgO gel liquid is dried to obtain a green body, which is then dehydrated at 50-160 ° C and then heated to 500 ° C for degreasing;

[0013] S4. The degreased green body is heated to 1400-1450° C. for sintering, and after cooling, a MgO ceramic material prepared by low-temperature sintering is obtained.

[0014] Furthermore, the mixed powder is pre-treated by acid solution impurity removal and ball milling, which can effectively remove oxides in the original powder that affect the thermal conductivity of the material, improve the surface energy and sintering activity of the powder, and increase the uniformity of the mixing of MgO powder and sintering aid.

[0015] Further, the acidic solution includes HNO 3 , HCl, H 2 SO 4 , acetic acid, and the solution concentration is 2-5%.

[0016] Furthermore, the mass ratio of the mixed powder to the organic matter is 2.5 to 3:1.

[0017] Furthermore, the organic matter includes a monomer, a cross-linking agent, a dispersant and a catalyst, and the mass ratio thereof is 8:2:1:1.

[0018] Furthermore, the monomer is one or more of acrylic acid, dimethylacrylamide, dimethylaminomethacrylate, methacrylate, and hydroxyethyl acrylate; the crosslinking agent is one or more of N,N-methyleneacrylamide and isocyanate; the catalyst is one or more of tetramethylethylenediamine, Lewis acid, and polyacrylamide.

[0019] Furthermore, the dehydration treatment includes heat preservation at 50° C., 80° C., 120° C. and 160° C. for 2 to 3 hours respectively.

[0020] Furthermore, during the heating and degreasing process, the temperature is kept at 500° C. for 2 to 3 hours.

[0021] Furthermore, the heating rate of the dehydration treatment is 5 to 10°C / min; the heating rate of the heating degreasing is 1 to 5°C / min.

[0022] Furthermore, the sintering heating rate is 1-5°C / min, and the holding time is 2-3h.

[0023] Compared with the prior art, the beneficial effects are:

[0024] The present invention adds Al into MgO ceramics 2 O 3 and MgF 2 , using MgF 2 Lowering the melting point of the mixture, and Al 2 O 3 It can improve the sintering performance of MgO ceramics by solid solution, reduce the number and size of pores and MgF 2 It can also reduce MgAl 2 O 4 Phase formation temperature, MgAl 2 O 4 Phase can replace Al 2 O 3 Filling between MgO grains makes the particles more compact. The two work together to significantly reduce the firing temperature of MgO ceramics.

[0025] The present invention mixes raw materials such as MgO with polymer monomers, obtains MgO gel liquid by cross-linking, and obtains an embryo body after drying, which effectively ensures the dispersion of MgO and avoids the agglomeration of MgO. Through the matching of raw materials, the temperature of the present invention is controlled at 1400-1450°C for sintering, and MgO ceramics with excellent mechanical properties and good thermal conductivity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 SEM images of the sintered samples (a) 3% MgF 2 SEM image at 1400℃; (b) 4%MgF 2 SEM image at 1400℃; (c) 5%MgF 2 SEM image at 1400℃; (d) 3% MgF 2 SEM image at 1450℃; (e) 4%MgF 2 SEM image at 1450℃; (f) 5% MgF 2 SEM image at 1450°C.

[0027] Figure 2 This is the XRD pattern of the sample sintered at 1400℃.

[0028] Figure 3This is the XRD pattern of the sample sintered at 1450℃. DETAILED DESCRIPTION

[0029] The following is further explained and illustrated in conjunction with the examples, but the specific examples do not limit the present invention in any form. If not specifically stated, the methods and equipment used in the examples are conventional methods and equipment in the art, and the raw materials used are all conventional commercially available raw materials.

[0030] Example 1

[0031] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0032] S1. Preprocessing

[0033] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:3 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0034] S2. Preparation of gel solution

[0035] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0036] S3. Drying and molding

[0037] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0038] S4. Dehydration and degreasing

[0039] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0040] S5. Sintering

[0041] Finally, the temperature was raised from 500°C to 1000°C at 5°C / min and kept at that temperature for 20 min, and then raised from 1000°C to 1400°C at 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain MgO ceramic material prepared by low-temperature sintering.

[0042] Example 2

[0043] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0044] S1. Preprocessing

[0045] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:4 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0046] S2. Preparation of gel solution

[0047] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0048] S3. Drying and molding

[0049] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0050] S4. Dehydration and degreasing

[0051] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0052] S5. Sintering

[0053] Finally, the temperature was raised from 500°C to 1000°C at 5°C / min and kept at that temperature for 20 min, and then raised from 1000°C to 1400°C at 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain MgO ceramic material prepared by low-temperature sintering.

[0054] Example 3

[0055] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0056] S1. Preprocessing

[0057] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:5 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0058] S2. Preparation of gel solution

[0059] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0060] S3. Drying and molding

[0061] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0062] S4. Dehydration and degreasing

[0063] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0064] S5. Sintering

[0065] Finally, the temperature was raised from 500°C to 1000°C at 5°C / min and kept at that temperature for 20 min, and then raised from 1000°C to 1400°C at 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain MgO ceramic material prepared by low-temperature sintering.

[0066] Example 4

[0067] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0068] S1. Preprocessing

[0069] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:3 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0070] S2. Preparation of gel solution

[0071] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter containing monomers, cross-linking agents, dispersants, and catalysts in a ratio of 3:1, wherein the mass ratio of monomers, cross-linking agents, dispersants, and catalysts is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0072] S3. Drying and molding

[0073] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0074] S4. Dehydration and degreasing

[0075] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0076] S5. Sintering

[0077] Finally, the temperature was increased from 500°C to 1000°C at a rate of 5°C / min and kept at that temperature for 20 min, and then increased from 1000°C to 1450°C at a rate of 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain the MgO ceramic material prepared by low-temperature sintering.

[0078] Example 5

[0079] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0080] S1. Preprocessing

[0081] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:4 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0082] S2. Preparation of gel solution

[0083] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with monomers, crosslinking agents, dispersants, and catalysts according to a certain ratio, and the mixed slurry is vacuum-treated to obtain MgO gel liquid.

[0084] S3. Drying and molding

[0085] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0086] S4. Dehydration and degreasing

[0087] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0088] S5. Sintering

[0089] Finally, the temperature was increased from 500°C to 1000°C at a rate of 5°C / min and kept at that temperature for 20 min, and then increased from 1000°C to 1450°C at a rate of 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain the MgO ceramic material prepared by low-temperature sintering.

[0090] Example 6

[0091] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0092] S1. Preprocessing

[0093] Magnesium oxide powder, aluminum oxide powder and magnesium fluoride powder are weighed and mixed in a mass percentage of 95:5:5 respectively, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0094] S2. Preparation of gel solution

[0095] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0096] S3. Drying and molding

[0097] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0098] S4. Dehydration and degreasing

[0099] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0100] S5. Sintering

[0101] Finally, the temperature was increased from 500°C to 1000°C at a rate of 5°C / min and kept at that temperature for 20 min, and then increased from 1000°C to 1450°C at a rate of 5°C / min and kept at that temperature for 3 h. The furnace was cooled to room temperature to obtain the MgO ceramic material prepared by low-temperature sintering.

[0102] Comparative Example 1

[0103] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0104] S1. Preprocessing

[0105] Magnesium oxide powder and magnesium fluoride powder with a mass percentage of 95:4 are weighed respectively and mixed, and then some impurities are removed in an acidic solution with a solution concentration of 2-5%, the surface activity of the mixed powder is increased, and the mixed powder is evenly dispersed.

[0106] S2. Preparation of gel solution

[0107] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0108] S3. Drying and molding

[0109] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0110] S4. Dehydration and degreasing

[0111] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50°C, 80°C, 120°C and 160°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours to dehydrate the green body. Then the temperature was raised from 160°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 2 hours for heating and degreasing.

[0112] S5. Sintering

[0113] Finally, the temperature was raised from 500°C to 1000°C at 5°C / min and kept at that temperature for 20 minutes, and then raised from 1000°C to 1400°C at 5°C / min and kept at that temperature for 170-190 minutes. The furnace was cooled to room temperature to obtain MgO ceramic material prepared by low-temperature sintering.

[0114] Comparative Example 2

[0115] This embodiment provides a MgO ceramic material prepared by low temperature sintering, the steps comprising:

[0116] S1. Preprocessing

[0117] Magnesium oxide powder and aluminum oxide powder are weighed and mixed in a mass percentage of 95:5, and then some impurities are removed in an acid solution with a solution concentration of 2-5%, so as to increase the surface activity of the mixed powder and make the mixed powder dispersed evenly.

[0118] S2. Preparation of gel solution

[0119] The mixed powder is mixed with anhydrous ethanol and ball-milled, and MgO powder is obtained by drying and sieving. The MgO powder is fully mixed with organic matter of monomer, cross-linking agent, dispersant and catalyst in a ratio of 3:1, wherein the mass ratio of monomer, cross-linking agent, dispersant and catalyst is 8:2:1:1, and then the mixed slurry is vacuumed to obtain MgO gel liquid.

[0120] S3. Drying and molding

[0121] The MgO gel liquid is poured into a mold and the mold is placed in an oven to dry the MgO gel liquid at 50° C. for 2 hours. The gel liquid undergoes a physical and chemical reaction in the corresponding mold to generate a green body with a certain strength.

[0122] S4. Dehydration and degreasing

[0123] The green body was placed in a muffle furnace, and the temperature was first raised from room temperature to 50℃, 80℃, 120℃ and 110℃ at a heating rate of 5℃ / min, and kept at this temperature for 3h respectively to dehydrate the green body. Then the temperature was raised from 110℃ to 500℃ at a heating rate of 1℃ / min and kept at this temperature for 2h for heating and degreasing.

[0124] S5. Sintering

[0125] Finally, the temperature was raised from 500°C to 1000°C at 5°C / min and kept at that temperature for 20 minutes, and then raised from 1000°C to 1400°C at 5°C / min and kept at that temperature for 170-190 minutes. The furnace was cooled to room temperature to obtain MgO ceramic material prepared by low-temperature sintering.

[0126] The MgO ceramic materials prepared in Examples 1 to 1 and Comparative Examples 1 and 2 were tested for performance, and the test results are shown in Table 1 below:

[0127] Table 1

[0128]

[0129] As can be seen from the table, in Al 2 O 3 and MgF 2 The two work together to prepare a magnesium oxide ceramic with a density of more than 90% at a low sintering temperature, and good thermal conductivity and strength. Figure 1 As shown in MgF 2 With the increase of the content of magnesium fluoride and the increase of sintering temperature, the density of the sample gradually increased, and the number and size of pores also decreased relatively. Figure 2 The magnesium aluminate phase was found in the MgO ceramics. The appearance of the magnesium aluminate phase reduced the number and size of pores in the MgO ceramics and increased the density of the sample.

[0130] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A MgO ceramic material prepared by low temperature sintering, characterized in that: The raw materials include magnesium oxide, aluminum oxide and magnesium fluoride, and the mass ratio of the magnesium oxide, aluminum oxide and magnesium fluoride is 95:5:3-5.

2. A method for preparing MgO ceramic material prepared by low temperature sintering, characterized in that: The preparation steps include: S1. The magnesium oxide, aluminum oxide and magnesium fluoride powders are mixed uniformly in a mass ratio to obtain a mixed powder; S2. The mixed powder is mixed with an organic matter to obtain a mixed slurry, and then the mixed slurry is vacuum treated to obtain a MgO gel liquid; S3. The MgO gel liquid is dried to obtain a green body, which is then dehydrated at 50 to 160 ° C and then heated to 500 ° C for degreasing; S4. The degreased green body is heated to 1400-1450° C. for sintering, and after cooling, a MgO ceramic material prepared by low-temperature sintering is obtained.

3. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: The mixed powder is also pre-treated by acid solution impurity removal and ball milling.

4. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: The mass ratio of the mixed powder to the organic matter is 2 to 4:

1.

5. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2 or 4, characterized in that: The organic matter includes monomers, cross-linking agents, dispersants and catalysts.

6. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 5, characterized in that: The monomer is one or more of acrylic acid, dimethyl acrylamide, dimethylamino methacrylate, methacrylate, and hydroxyethyl acrylate; the crosslinking agent is one or more of N,N-methylene acrylamide and isocyanate; and the catalyst is one or more of tetramethylethylenediamine, Lewis acid, and polyacrylamide.

7. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: The dehydration treatment includes heat preservation at 50° C., 80° C., 120° C. and 160° C. for 2 to 3 hours respectively.

8. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: During the heating degreasing process, the temperature is kept at 500° C. for 2 to 3 hours.

9. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: The heating rate of the dehydration treatment is 5-10°C / min; the heating rate of the heating degreasing is 1-5°C / min.

10. The method for preparing the MgO ceramic material prepared by low temperature sintering according to claim 2, characterized in that: The sintering heating rate is 1-5°C / min and the holding time is 2-3h.

Citation Information

Patent Citations

  • A high thermal conductivity oxide ceramic material and its preparation method

    CN104276815B

  • Method for preparing high-density magnesia ceramic

    CN102060514A

  • Y2O3-MgO nano-composite ceramic and preparation method thereof

    CN103922742A

  • High-transmittance high-purity aluminum oxynitride transparent ceramic and preparation method thereof

    CN107459354A

  • Porous sintered magnesia, batch for the production of a coarse ceramic refractory product with a grain size of sintered magnesia, such product as well as lining of an industrial furnace and industrial oven

    DE202017007171U1