Zirconia ceramic sintered gasket and preparation method thereof

By using an adhesive and a temperature-controlled casting process to prepare zirconia ceramic sintered gaskets, the problems of insufficient bending strength and density in existing technologies have been solved, and high-performance zirconia ceramic sintered gaskets have been prepared.

CN118930257APending Publication Date: 2024-11-12XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411295107.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies make it difficult to produce sintered zirconia ceramic gaskets with good flexural strength, roughness, and density.

Method used

A zirconia ceramic sintered gasket was prepared by using a binder and temperature-controlled casting process. YSZ powder, solvent, and dispersant were mixed and ball-milled. After adding the binder, the mixture was degassed and cast. Then, it was cut, dried, isostatically pressed, punched, and sintered. The casting temperature and sintering temperature were controlled.

Benefits of technology

The prepared zirconia ceramic sintered gasket has excellent bending strength, a smooth and dense surface, avoids warping and adhesion, ensures stable performance, and is suitable for electronic equipment and mechanical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045720140000081
    Figure BDA0005045720140000081
  • Figure BDA0005045720140000091
    Figure BDA0005045720140000091
Patent Text Reader

Abstract

The invention belongs to the field of ceramic chips, and discloses a zirconia ceramic sintered gasket preparation method, which comprises: carrying out ball milling, defoaming aging and casting on YSZ powder, a solvent, a dispersant and a glue to obtain a casting sheet; then drying, punching, degreasing, sintering and the like are carried out on the cast sheet to obtain a zirconia ceramic sintered gasket; wherein the YSZ powder is formed by mixing zirconium oxide powder and yttrium oxide powder according to the mass ratio of 92%: 8%, casting is temperature-zone temperature increasing casting, and the temperature of a first temperature zone is 30-45 DEG C; the temperature of the second temperature zone is 50-60 DEG C; the temperature of the first temperature zone is 65-70 DEG C, the temperature of the third temperature zone is 65-70 DEG C, the glue is prepared by mixing a plasticizer, a binder, toluene and isopropanol according to a certain mass ratio, the plasticizer is selected from at least one of tributyl phosphate and dibutyl phthalate, and the binder is selected from at least one of polymethyl methacrylate and polyvinyl alcohol. In addition, the invention further discloses the zirconia ceramic sintered gasket which is prepared through the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of ceramic sheets, and in particular to a zirconia ceramic sintered gasket and a preparation method thereof. Background Art

[0002] At present, zirconia ceramics are increasingly widely used in industrial and civilian fields. Since zirconia ceramics can be used in environmental conditions with high requirements for strength and toughness, zirconia ceramics are often used to make thin sheets, substrates, gaskets or other thin sheets.

[0003] These sheets can not only be used as structural components, such as in the fields of handicrafts and mechanical parts, but are also widely used in miniaturized electronic components of electronic equipment, such as flat oxygen sensors and circuit board substrates, as well as in ultra-large-scale integrated circuits. Therefore, these zirconia ceramic sheets have very broad application prospects.

[0004] Chinese patent application 201910481289.6 discloses a method for preparing a single-layer capacitor ceramic substrate, which includes the steps of batching, casting, lamination, lamination, cutting, pre-leveling, debinding, sintering, leveling, grinding and the like.

[0005] The ingredients in this scheme are composed of Class II porcelain powder, organic solvent, dispersant, adhesive and plasticizer, the debinding temperature is 400°C, and the sintering temperature is 1300±10°C.

[0006] Chinese patent application 202010544090.6 discloses a YSZ electrolyte preparation material, a cast sheet, a preparation method and a gas sensor, wherein the preparation method is as follows: the raw materials are mixed and ball-milled for 12 to 36 hours to obtain a mixture; the organic carrier and the organic auxiliary agent are added to the mixture, and the ball-milling is continued for 12 to 36 hours to obtain a pre-slurry; the pre-slurry is filtered through a 100 to 400 mesh filter, and a casting slurry is obtained after degassing for 1 to 5 hours and aging for 0.5 to 2 hours; the casting slurry is tape-cast to obtain the YSZ electrolyte.

[0007] The doping amount of yttrium oxide in the zirconium oxide in the scheme is 1-6%, and the drying temperature during the casting process is 40-110°C.

[0008] The problem that this scheme needs to solve: How to propose a preparation method for a sintered zirconia ceramic gasket with good performance. Summary of the invention

[0009] The purpose of this application is to propose a zirconia ceramic sintered gasket and a preparation method thereof, and to prepare a zirconia ceramic sintered gasket with excellent bending strength, roughness, density and other properties through a glue and a temperature zone casting process.

[0010] To achieve the above object, the present application discloses a method for preparing a sintered zirconia ceramic gasket, comprising the following steps:

[0011] Step 1: Mix YSZ powder, solvent and dispersant, and ball mill once to obtain a mixture;

[0012] Step 2: adding the glue to the mixture, and obtaining a cast sheet through secondary ball milling, degassing, aging, and casting;

[0013] Step 3: cutting, drying, isostatic pressing, punching, degreasing, and sintering the cast sheet to obtain a zirconia ceramic sintered gasket;

[0014] In step 1, the YSZ powder is composed of zirconium oxide powder and yttrium oxide powder mixed in a mass ratio of 93% to 91%: 7% to 9%;

[0015] In step 2, the casting is performed in temperature zones with increasing temperature, wherein the temperature in the first temperature zone is 30-45°C; the temperature in the second temperature zone is 50-60°C; and the temperature in the third temperature zone is 65-70°C.

[0016] Preferably, the adhesive is prepared by mixing a plasticizer, a binder, toluene and isopropanol, and the mass ratio of the plasticizer, the binder, toluene and the isopropanol is 2.2-2.5: 0.7-0.8: 0.4-0.6: 1-1.2;

[0017] The mass ratio of the adhesive to the YSZ powder is 30-35:50-60.

[0018] Preferably, the plasticizer is selected from at least one of tributyl phosphate and dibutyl phthalate;

[0019] The binder is selected from at least one of polymethyl methacrylate and polyvinyl alcohol.

[0020] Preferably, the solvent is selected from at least one of toluene and isopropanol, and the mass ratio of the solvent to the YSZ powder is 27-33:50-60;

[0021] More preferably, the solvent is a mixture of toluene and isopropanol in a mass ratio of 4:1.

[0022] The dispersant is selected from at least one of polyacrylamide and sodium polyacrylate, and the mass ratio of the dispersant to the YSZ powder is 1-1.5:50-60.

[0023] Preferably, in the casting process of step 2, the casting rate is 0.2-0.3 m / min, the casting time in the first temperature zone is 15 min; the casting time in the second temperature zone is 10 min; and the casting time in the third temperature zone is 5 min.

[0024] Preferably, the ball milling process is: add 10mm, 15mm, 20mm zirconium beads 12KG in total, wherein the mass ratio of 10mm, 15mm, 20mm zirconium beads is 4:5:3, the first ball milling is 20h, the second ball milling is 15h, and the ball milling speed is 300rpm

[0025] Preferably, the isostatic pressing step of step 3 is: stacking the cast sheet on a sheet glass plate, vacuum-sealing it with a plastic bag, and then placing it in an isostatic press, isostatically pressing it at a pressure of 60Mpa to 80Mpa and at 50 to 60°C for 30 to 45 minutes.

[0026] Preferably, the degreasing step of step 3 is: stack 5 to 8 cast sheets, place them on an alumina support plate, cover them with a layer of ceramic refractory gasket, and then increase the temperature to 300 to 500° C. at 1 to 2° C. / min, and keep them warm for 16 to 24 hours.

[0027] Preferably, the sintering step in step 3 is: increasing the temperature to 1200-1500° C. at 5-8° C. / min, and keeping the temperature for 16-24 hours;

[0028] More preferably, the sintering temperature is 1400-1500°C.

[0029] In addition, a zirconia ceramic sintered gasket is also disclosed, which is prepared by the above-mentioned preparation method of the zirconia ceramic sintered gasket.

[0030] The beneficial effects of this application are:

[0031] The present application provides a method for preparing a sintered zirconia ceramic gasket. By using a glue prepared by mixing a plasticizer and a binder, the viscosity and fluidity of the slurry can be improved, so that the embryo obtained by casting has good toughness and uniformity; then, through the temperature zone casting process, the solvent in the slurry is uniformly volatilized to obtain a green embryo belt with a smooth and dense surface, and then the embryo is processed by an isostatic pressing process to make the embryo more dense and flat, and then the sintered zirconia ceramic gasket with good bending strength, roughness and density is obtained by degreasing and sintering. The superior bending strength can well adapt to and prevent the warping of the ceramic sheet, and will not break in the process, and will not have a counter-effect on the sintering. At the same time, its higher roughness can prevent it from adhering to the sintered zirconia ceramic sheet. At the same time, it is close to the composition of the zirconia ceramic sheet and has a higher density. As a sintered gasket, it can effectively avoid the introduction of other impurity elements and affect the performance of the zirconia ceramic sheet. DETAILED DESCRIPTION

[0032] In the description of this application, it should be noted that if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0033] Example 1

[0034] Step 1: Mix YSZ powder, solvent and polyacrylamide in a mass ratio of 55:30:1.3, add 10 mm, 15 mm and 20 mm zirconium beads in a total of 12 kg, wherein the mass ratio of 10 mm, 15 mm and 20 mm zirconium beads is 4:5:3, and ball mill for 20 hours at a ball milling speed of 300 rpm to obtain a mixture;

[0035] Step 2: Add the glue to the mixture at a mass ratio of 33:55 with the YSZ powder in step 1, perform secondary ball milling for 15 hours at a ball milling speed of 300 rpm, then degas for 1 hour, age for 5 hours, and then perform temperature-increasing casting in different temperature zones at a rate of 0.3 m / min, wherein the temperature in the first temperature zone is 38°C and the casting time is 15 minutes; the temperature in the second temperature zone is 55°C and the casting time is 10 minutes; the temperature in the third temperature zone is 68°C and the casting time is 5 minutes, to obtain a cast sheet;

[0036] Step 3: Dry the cast sheet at 100°C, isostatically press at 70Mpa, 55°C for 38min, and then punch it; then stack 5 sheets, place them on an alumina support plate, cover them with a layer of ceramic refractory gasket, and then degrease at 400°C at 1.5°C / min, keep warm for 20h, and finally sinter at 1450°C at 7°C / min, keep warm for 20h to obtain a zirconia ceramic sintered gasket;

[0037] The YSZ powder is composed of zirconium oxide powder and yttrium oxide powder, and the mass ratio of the zirconium oxide powder to the yttrium oxide powder is 92:8.

[0038] The solvent is a mixture of toluene and isopropanol in a mass ratio of 4:1;

[0039] The adhesive is prepared by mixing tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol in a mass ratio of 2.3:0.75:0.5:1.1.

[0040] Example 2

[0041] Step 1: Mix YSZ powder, solvent and polyacrylamide in a mass ratio of 50:33:1, add 10mm, 15mm and 20mm zirconium beads (12 kg in total), wherein the mass ratio of 10mm, 15mm and 20mm zirconium beads is 4:5:3, and ball mill for 20 hours at a ball milling speed of 300 rpm to obtain a mixture;

[0042] Step 2: Add the glue to the mixture at a mass ratio of 35:50 with the YSZ powder in step 1, perform secondary ball milling for 15 hours at a ball milling speed of 300 rpm, then degas for 1 hour, age for 5 hours, and then perform temperature-increasing casting in different temperature zones at a rate of 0.3 m / min, wherein the temperature in the first temperature zone is 38°C and the casting time is 15 minutes; the temperature in the second temperature zone is 55°C and the casting time is 10 minutes; the temperature in the third temperature zone is 68°C and the casting time is 5 minutes, to obtain a cast sheet;

[0043] Step 3: Dry the cast sheet at 100°C, isostatically press at 60Mpa, 50°C for 45 minutes, and then punch it; then stack 5 sheets, place them on an alumina support plate, cover them with a layer of ceramic refractory gasket, and then degrease at 300°C at 1°C / min, keep warm for 20 hours, and finally sinter at 1400°C at 5°C / min, keep warm for 20 hours to obtain a zirconia ceramic sintered gasket;

[0044] The YSZ powder is composed of zirconium oxide powder and yttrium oxide powder, and the mass ratio of the zirconium oxide powder to the yttrium oxide powder is 92:8.

[0045] The solvent is a mixture of toluene and isopropanol in a mass ratio of 4:1;

[0046] The adhesive is prepared by mixing tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol in a mass ratio of 2.3:0.75:0.5:1.1.

[0047] Example 3

[0048] Step 1: Mix YSZ powder, solvent and polyacrylamide in a mass ratio of 60:27:1.5, add 10mm, 15mm and 20mm zirconium beads (12 kg in total), wherein the mass ratio of 10mm, 15mm and 20mm zirconium beads is 4:5:3, and ball mill for 20 hours at a ball milling speed of 300 rpm to obtain a mixture;

[0049] Step 2: Add the glue to the mixture at a mass ratio of 30:60 with the YSZ powder in step 1, perform secondary ball milling for 15 hours at a ball milling speed of 300 rpm, then degas for 1 hour, age for 5 hours, and then perform temperature-increasing casting in different temperature zones at a rate of 0.3 m / min, wherein the temperature in the first temperature zone is 38°C and the casting time is 15 minutes; the temperature in the second temperature zone is 55°C and the casting time is 10 minutes; the temperature in the third temperature zone is 68°C and the casting time is 5 minutes, to obtain a cast sheet;

[0050] Step 3: Dry the cast sheet at 100°C, isostatically press at 80Mpa, 60°C for 30min, and then punch it; then stack 5 sheets, place them on an alumina support plate, cover them with a layer of ceramic refractory gasket, and then degrease at 500°C at 2°C / min, keep warm for 20h, and finally sinter at 1500°C at 8°C / min, keep warm for 20h to obtain a zirconia ceramic sintered gasket;

[0051] The YSZ powder is composed of zirconium oxide powder and yttrium oxide powder, and the mass ratio of the zirconium oxide powder to the yttrium oxide powder is 92:8.

[0052] The solvent is a mixture of toluene and isopropanol in a mass ratio of 4:1;

[0053] The adhesive is prepared by mixing tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol in a mass ratio of 2.3:0.75:0.5:1.1.

[0054] Example 4

[0055] The method is basically the same as Example 1, except that the mass ratio of tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol in the adhesive is 2.2:0.7:0.6:1.2.

[0056] Example 5

[0057] The method is basically the same as Example 1, except that the mass ratio of tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol in the adhesive is 2.5:0.8:0.4:1.

[0058] Example 6

[0059] The method is basically the same as Example 1, except that the plasticizer is dibutyl phthalate.

[0060] Example 7

[0061] It is basically the same as Example 1, except that the binder is polymethyl methacrylate.

[0062] Example 8

[0063] It is basically the same as Example 1, except that, during the casting process, the temperature of the first temperature zone is 30°C, the temperature of the second temperature zone is 50°C, and the temperature of the third temperature zone is 65°C.

[0064] Example 9

[0065] It is basically the same as Example 1, except that, during the casting process, the temperature of the first temperature zone is 45°C, the temperature of the second temperature zone is 60°C, and the temperature of the third temperature zone is 70°C.

[0066] Example 10

[0067] It is basically the same as Example 1, except that the sintering temperature during the sintering process is 1300°C.

[0068] Embodiment 11

[0069] It is basically the same as Example 1, except that the sintering temperature during the sintering process is 1100°C.

[0070] Example 12

[0071] It is basically the same as Example 1, except that the sintering temperature during the sintering process is 1550°C.

[0072] Comparative Example 1

[0073] The method is basically the same as Example 1, except that the mass ratio of zirconium oxide powder to yttrium oxide powder in the YSZ powder is 93%:7%.

[0074] Comparative Example 2

[0075] The method is basically the same as Example 1, except that the mass ratio of zirconium oxide powder to yttrium oxide powder in the YSZ powder is 91%:9%.

[0076] Comparative Example 3

[0077] The method is basically the same as Example 1, except that the casting process is performed at 50° C. throughout the casting process.

[0078] Comparative Example 4

[0079] It is basically the same as Example 1, except that during the casting process, the temperature of the first temperature zone is 48°C, the temperature of the second temperature zone is 63°C, and the temperature of the third temperature zone is 80°C.

[0080] Comparative Example 5

[0081] It is basically the same as Example 1, except that, during the casting process, the temperature of the first temperature zone is 68°C, the temperature of the second temperature zone is 55°C, and the temperature of the third temperature zone is 38°C.

[0082] Comparative Example 6

[0083] The method is basically the same as Example 1, except that glycerol is used to replace tributyl phosphate in the glue.

[0084] Comparative Example 7

[0085] The method is substantially the same as Example 1, except that hydroxypropyl methylcellulose is used to replace the polyvinyl alcohol in the glue.

[0086] Comparative Example 8

[0087] The method is basically the same as Example 1, except that the adhesive does not contain tributyl phosphate and polyvinyl alcohol.

[0088] Comparative Example 9

[0089] The method is basically the same as Example 1, except that in step 2, tributyl phosphate, polyvinyl alcohol, toluene and isopropyl alcohol are not pre-mixed to prepare a glue, but are directly added to the mixture in step 1.

[0090] Performance Test:

[0091] Bending strength: Bending strength tester is used to test the bending strength.

[0092] Surface roughness: Use a roughness meter to test 5 random points on the ceramic surface and take the average value

[0093] Density: Density is measured using Archimedes' principle

[0094] The test results are shown in Table 1:

[0095] Table 1

[0096]

[0097]

[0098] Result analysis:

[0099] 1. It can be seen from Examples 1-3 that when the raw material ratio in step 1 and the isostatic pressing operation, degreasing operation, and sintering operation in step 3 are changed, the performance of the zirconia ceramic sintered gasket will be affected to a certain extent;

[0100] However, it can be seen from observation of Examples 10-12 that when the sintering temperature is between 1200 and 1400°C, the degree of crystallization of the ceramic sintered gasket will decrease during sintering, thereby reducing the performance of the gasket; when the sintering temperature is lower than 1200°C, the degree of crystallization inside the gasket is very low, the ceramic formation is incomplete, and it cannot be used in production; when the sintering temperature is at 1500°C, the gasket has been completely sintered, and further heating will increase the sintering cost, and over-sintering may cause the gasket performance to deteriorate.

[0101] 2. It can be seen from Example 1 and Comparative Examples 1-2 that the addition of yttrium oxide powder is to improve the stability of the material. Therefore, when the yttrium oxide content in the YSZ powder is lower than 8%, the slurry system in this case is not stable and cannot be solidified during the casting process; when it is higher than 8%, the casting slurry system is still unstable. Although the casting process can be completed, it affects the crystal growth inside the gasket during the sintering process, resulting in uneven wrinkles on the surface of the gasket, which cannot be used in production.

[0102] 3. It can be seen from Example 1, Examples 4-5 and Comparative Examples 8-9 that when the content of plasticizer and binder in the glue changes, it will affect the relative density and bending strength of the gasket during the casting process; and from Comparative Example 8, it can be seen that the plasticizer and binder in the glue are indispensable. Without them, the viscosity of the casting slurry is too low and cannot be cast normally; from Comparative Example 9, it can be seen that when the plasticizer and binder are not mixed into the glue in advance but are directly added to the raw materials, the difficulty of dispersing the raw materials increases, affecting the uniformity of the casting slurry, resulting in a decrease in the performance of the gasket after sintering.

[0103] 4. It can be seen from Example 1 and Examples 6-7 that tributyl phosphate in the plasticizer has a certain defoaming effect, and polyvinyl alcohol in the binder has a better film-forming effect on the cast sheet. Therefore, when the two are used in combination, a cast sheet with better uniformity and toughness can be obtained for sintering, and a sintered gasket with better performance can be obtained. Moreover, after using dibutyl phthalate or polymethyl methacrylate to replace the plasticizer or binder, although the performance of the sintered gasket will be reduced, it can also meet the application requirements.

[0104] In Comparative Examples 6-7, when the plasticizer glycerol or the binder hydroxypropyl methylcellulose was used for corresponding replacement, the internal uniformity and toughness of the cast slurry prepared by the plasticizer glycerol were relatively poor, the sintered gaskets prepared could not be used in production, and the glue prepared by the binder hydroxypropyl methylcellulose could not be added to the system for dispersion. It can be seen that not all plasticizers or binders can achieve the effect of this case.

[0105] 5. It can be seen from Example 1, Examples 8-9 and Comparative Examples 3-5 that the temperature zone casting process can make the solvent in the slurry evaporate evenly during the casting process to obtain a green embryo belt with a smooth and dense surface. Therefore, when the casting is performed at a uniform temperature throughout the process, the slurry is heated too quickly in the front process, resulting in surface film formation, which affects the volatilization of the solvent in the back process, resulting in the cast sheet still containing solvent, affecting the performance of the sintered gasket; and when the temperature of each temperature zone exceeds the range, due to the high temperature, the solvent will evaporate too quickly, and excessive casting will cause cracks in the cast sheet; when the process of heating up first and then cooling down is adopted, the temperature in the front process is too high, and the surface of the casting slurry solidifies quickly, resulting in the internal solvent being unable to volatilize, and wrinkles and cracks appear on the surface of the cast sheet, making it unusable.

[0106] The above embodiments are preferred implementation modes of the present application, but the implementation modes of the present application are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present application shall be equivalent replacement methods and shall be included in the protection scope of the present application.

Claims

1. A method for preparing a zirconia ceramic sintered gasket, characterized in that: The preparation method comprises the following steps: Step 1: Mix YSZ powder, solvent and dispersant, and ball mill once to obtain a mixture; Step 2: adding the glue to the mixture, and obtaining a cast sheet through secondary ball milling, degassing, aging, and casting; Step 3: cutting, drying, isostatic pressing, punching, degreasing, and sintering the cast sheet to obtain a zirconia ceramic sintered gasket; In step 1, the YSZ powder is composed of zirconium oxide powder and yttrium oxide powder mixed in a mass ratio of 92%:8%; The casting in step 2 is a casting with increasing temperature in different temperature zones, wherein the temperature in the first temperature zone is 30-45°C; the temperature in the second temperature zone is 50-60°C; and the temperature in the third temperature zone is 65-70°C; The adhesive is prepared by mixing a plasticizer, a binder, toluene and isopropanol, and the mass ratio of the plasticizer, the binder, the toluene and the isopropanol is 2.2-2.5: 0.7-0.8: 0.4-0.6: 1-1.2; The plasticizer is selected from at least one of tributyl phosphate and dibutyl phthalate; The binder is selected from at least one of polymethyl methacrylate and polyvinyl alcohol.

2. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: The mass ratio of the adhesive to the YSZ powder is 30-35:50-60.

3. The method for preparing a sintered zirconium oxide ceramic gasket according to claim 2, characterized in that The solvent is selected from at least one of toluene and isopropanol, and the mass ratio of the solvent to the YSZ powder is 27-33:50-60; The dispersant is selected from at least one of polyacrylamide and sodium polyacrylate, and the mass ratio of the dispersant to the YSZ powder is 1-1.5:50-60.

4. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: During the casting process of step 2, the casting rate is 0.2-0.3 m / min, the casting time in the first temperature zone is 15 min; the casting time in the second temperature zone is 10 min; and the casting time in the third temperature zone is 5 min.

5. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: The ball milling process is as follows: adding 12 kg of 10 mm, 15 mm and 20 mm zirconium beads, wherein the mass ratio of the 10 mm, 15 mm and 20 mm zirconium beads is 4:5:3, the first ball milling is for 20 hours, the second ball milling is for 15 hours, and the ball milling speed is 300 rpm.

6. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: The isostatic pressing step of step 3 is as follows: stacking the cast sheet on a sheet glass plate, vacuum-packaging it with a plastic bag, and then placing it in an isostatic press for 30 to 45 minutes at a pressure of 60 MPa to 80 MPa and at 50 to 60° C.

7. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: The degreasing step of step 3 is as follows: stack 5 to 8 cast sheets, place them on an alumina support plate, cover them with a layer of ceramic refractory gasket, and then increase the temperature to 300 to 500° C. at 1 to 2° C. / min, and keep them warm for 16 to 24 hours.

8. The method for preparing a sintered zirconia ceramic gasket according to claim 1, characterized in that: The sintering step of step 3 is: increasing the temperature to 1200-1500° C. at 5-8° C. / min and keeping the temperature for 16-24 hours.

9. A zirconia ceramic sintered gasket, characterized in that: The sintered zirconium oxide ceramic gasket is prepared by the preparation method of any one of claims 1 to 8.

Citation Information

Patent Citations

  • Metal oxide casting

    CA963669A

  • Preparation method of zirconium oxide ceramic for oxygen sensor

    CN104891969A

  • Zirconia ceramic fingerprint identification sheet and preparing and application method thereof

    CN106495691A

  • Method for preparing zirconia ceramic piece through in-situ curtain coating

    CN107399969A

  • Zirconium oxide ceramic and preparation method thereof

    CN107445612A