Method for preparing high-density PZT ceramic through powder slurry pouring

Preparation of PZT ceramics by slurry casting method solves the problems of uneven ceramic structure and low density in the prior art, and achieves high density, low cost and suitable for mass production.

CN118930259APending Publication Date: 2024-11-12GUIZHOU ZHENHUA HONGYUN ELECTRONICS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411066699.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing PZT ceramic molding methods have problems such as uneven structure, low density, high production costs, complex operation and difficult to adapt to mass production.

Method used

By using the slurry casting method, PZT porcelain material is prepared by mixing Pb3O4, ZrO2 and TiO2, and mixed with deionized water, dispersant and binder, ball milled to the appropriate particle size, injected into the gypsum mold and then sintered in a sintering furnace. , control the sintering conditions to achieve high density.

Benefits of technology

The microstructure of PZT ceramics is uniform, dense, low production cost, simple operation, suitable for mass production, and low requirements for mold accuracy, which does not affect the purity of the ceramic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930259A_ABST
    Figure CN118930259A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing PZT ceramic, and aims to provide a method for preparing high-density PZT ceramic through powder slurry pouring, wherein the method is uniform in material structure, high in density, simple in production process, easy to operate and control, high in production efficiency and low in production cost. According to the technical scheme, the preparation method comprises the following steps: uniformly mixing Pb3O4, ZrO2 and TiO2, and respectively preparing PZT porcelain with Zr / Ti = 0.92, 1, 1.08, 5.67 and 19 by adopting a solid phase method; adding deionized water and a dispersing agent, mixing, and carrying out ball milling until the particle size is less than or equal to 200 microns; adding a binder, uniformly stirring, injecting into a mold under pressure, molding, demolding, and drying to obtain a green body of which the relative density is greater than 50%; heating the green body to 400-750 DEG C at the rate of 0.5-1 DEG C / min, and discharging the rubber for 4-6 hours; and heating to 1200-1300 DEG C at a rate of 3-5 DEG C / min, and carrying out lead-buried sintering for 1-4 hours to obtain the PZT ceramic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a piezoelectric ceramic material, and in particular to a method for preparing a high-density PZT ceramic based on a slurry casting method. Background Art

[0002] It is well known that the higher the density of PZT ceramics (relative density ≥ 95.0%) and the more uniform the structure, the better the performance of the piezoelectric transducer device will be.

[0003] At present, there are two main methods for PZT ceramic molding: compression molding and isostatic pressing. Compression molding, whether it is unidirectional pressing or bidirectional pressing, will have defects such as uneven PZT ceramic structure, easy stratification during the compression molding process, low density (relative density of about 90.0%), and high precision requirements for molds and presses. Although the static pressing method can solve the problems of uniform ceramic structure and low shrinkage, the production cost is high, and the ceramic material must be granulated before pressing; the operation is complicated and difficult to adapt to mass production. In addition, there is also a gel injection molding method that can be used to prepare other ceramic materials, but this method requires the addition of many additives to complete the green body molding, which will affect the purity and density of the ceramic material. Summary of the invention

[0004] In view of the above-mentioned defects existing in the prior art, the present invention aims to provide a method for preparing high-density PZT ceramics by slurry casting, which has uniform material structure, high density, simple production process, easy operation and control, high production efficiency and low production cost.

[0005] In order to achieve the above object, the method provided by the present invention adopts the following technical solutions:

[0006] 1) Pb3O4, ZrO2 and TiO2 were uniformly mixed and prepared into PZT ceramic materials with Zr / Ti=0.92, 1, 1.08, 5.67 and 19 respectively by solid phase method;

[0007] 2) mixing the PZT ceramic material with deionized water and a dispersant, and ball-milling the mixture to obtain a slurry with a particle size of ≤200 μm;

[0008] 3) Adding a binder to the slurry, stirring evenly, and injecting it into a plaster mold at a pressure of 0.08-0.15Mpa, demoulding and drying after molding to obtain a green body with a relative density greater than 50%;

[0009] 4) placing the green body in a sintering furnace, heating it to 400-750°C at a rate of 0.5-1°C / min, and debinding for 4-6 hours; then heating it to 1200-1300°C at a rate of 3-5°C / min in an air atmosphere, burying it with lead and sintering it for 1-4 hours to obtain PZT ceramics.

[0010] In the above technical solution, the amount of deionized water added is 20-30wt% of the total amount of the PZT ceramic material.

[0011] In the above technical solution, the dispersant is ammonium polyacrylate, and the added amount thereof is 0.5-1.5wt% of the total amount of the PZT ceramic material.

[0012] In the above technical solution, the binder is polyvinyl alcohol, and the amount added is 0.5-5wt% of the total amount of the PZT ceramic material.

[0013] In the above technical solution, the rotation speed of the ball mill is 2000-2500 r / min; the ball milling medium is zirconia balls with a particle size of 0.3 mm.

[0014] In the above technical solution, the drying method described in step 3) is: first place the demoulded green body in a room temperature environment of 20-30°C for drying for 3 days, and then transfer it to a 60°C oven for drying for 24 hours.

[0015] Compared with the prior art, the method of the present invention is

[0016] 1. The PZT ceramic prepared by the present invention has a uniform microstructure and high density, and the relative density is ≥95%.

[0017] 2. The PZT ceramic green body prepared by the present invention shrinks evenly, does not deform, crack or delaminate, and has low requirements on mold precision.

[0018] 3. The present invention adopts a slurry casting method with few additives and does not affect the purity of the PZT ceramic.

[0019] 4. The process of the present invention is simple to operate, easy to control, low in cost, and suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the distribution diagram of the particle size of ball mill slurry;

[0021] Figure 2 It is the XRD diffraction pattern of PZT ceramics prepared by the method of the present invention;

[0022] Figure 3 This is a SEM scan of the PZT ceramics prepared by the method of the present invention.

[0023] from Figure 1 It can be seen that by controlling the process variables, the particle size range of the ball milling slurry can reach 0.1 to 0.5 microns, and the particle size is more uniform.

[0024] from Figure 2It can be seen that the PZT ceramic provided by the present invention is a single perovskite structure, which provides a guarantee for the stable performance of the product.

[0025] from Figure 3 It can be seen that the PZT ceramic provided by the present invention has a more uniform crystal structure, is free of defects, and has a high density. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments:

[0027] Example 1

[0028] 1) Pb3O4 with a purity of ≥98%, ZrO2 with a purity of ≥99%, and TiO2 with a purity of ≥99% are prepared into a 1kg mixture according to Zr / Ti=0.92;

[0029] 2) preparing the PZT ceramic material by a solid phase method;

[0030] 3) The PZT ceramic material is mixed evenly with 200 ml of deionized water and 15 g of ammonium polyacrylate, and ball-milled to a slurry with a particle size of ≤ 200 μm; the speed of the ball mill is controlled to be 2000 r / min, and the ball milling medium is a zirconia ball with a particle size of 0.3 mm;

[0031] 4) adding 30 g of polyvinyl alcohol to the slurry, stirring at a speed of 120 r / min for 30 min; then injecting into a plaster mold at a pressure of 0.15 MPa, and demolding after solidification to obtain a wet blank;

[0032] 5) drying the wet blank at room temperature (25° C.) for 3 days, and then drying it in an oven at 60° C. for 24 hours to obtain a green blank having a relative density greater than 50%;

[0033] 6) placing the green body in a sintering furnace, heating it to 600°C at a rate of 0.5°C / min, and debinding for 5 hours; then heating it to 1250°C at a rate of 3°C / min in an air atmosphere, sintering it with lead for 2 hours, and obtaining a PZT ceramic with a relative density of 96%.

[0034] Example 2

[0035] 1) Pb3O4 with a purity of ≥98%, ZrO2 with a purity of ≥99%, and TiO2 with a purity of ≥99% are prepared into a 1kg mixture according to Zr / Ti=0.92;

[0036] 2) preparing the PZT ceramic material by a solid phase method;

[0037] 3) The PZT ceramic material is mixed evenly with 300 ml of deionized water and 5 g of ammonium polyacrylate, and ball-milled to a slurry with a particle size of ≤ 200 μm; the speed of the ball mill is controlled to be 2300 r / min, and the ball milling medium is a zirconia ball with a particle size of 0.3 mm;

[0038] 4) adding 20 g of polyvinyl alcohol to the slurry, stirring at a speed of 120 r / min for 30 min; then injecting into a plaster mold at a pressure of 0.08 MPa, and demolding after solidification to obtain a wet blank;

[0039] 5) drying the wet blank at room temperature (25° C.) for 3 days, and then drying it in an oven at 60° C. for 24 hours to obtain a green blank having a relative density greater than 50%;

[0040] 6) placing the green body in a sintering furnace, heating it to 600°C at a rate of 1°C / min, and debinding for 5 hours; then heating it to 1250°C at a rate of 5°C / min in an air atmosphere, sintering it with lead for 2 hours, and obtaining a PZT ceramic with a relative density of 95.8%.

[0041] Example 3

[0042] 1) Pb3O4 with a purity of ≥98%, ZrO2 with a purity of ≥99%, and TiO2 with a purity of ≥99% are prepared into a 1kg mixture according to Zr / Ti=0.92;

[0043] 2) preparing the PZT ceramic material by a solid phase method;

[0044] 3) The PZT ceramic material is mixed evenly with 250 ml of deionized water and 10 g of ammonium polyacrylate, and ball-milled to a slurry with a particle size of ≤ 200 μm; the speed of the ball mill is controlled to be 2500 r / min, and the ball milling medium is a zirconia ball with a particle size of 0.3 mm;

[0045] 4) adding 20 g of polyvinyl alcohol to the slurry, stirring at a speed of 120 r / min for 15 min; then injecting into a plaster mold at a pressure of 0.12 Mpa, and demolding after solidification to obtain a wet blank;

[0046] 5) drying the wet blank at room temperature (25° C.) for 3 days, and then drying it in an oven at 60° C. for 24 hours to obtain a green blank having a relative density greater than 50%;

[0047] 6) placing the green body in a sintering furnace, heating it to 600°C at a rate of 0.8°C / min, and debinding for 5 hours; then heating it to 1250°C at a rate of 4°C / min in an air atmosphere, sintering it with lead for 2 hours, and obtaining a PZT ceramic with a relative density of 96.2%.

[0048] Example 4

[0049] In step 1), Zr / Ti=1, and the other steps can be the same as in Example 1. The relative density of the PZT ceramic prepared in this example is 95.7%.

[0050] Example 5

[0051] In step 1), Zr / Ti=1, and the other steps can be the same as those in Example 2. The relative density of the PZT ceramic prepared in this example is 97.1%.

[0052] Example 6

[0053] In step 1), Zr / Ti=1, and the other steps can be the same as those in Example 3. The relative density of the PZT ceramic prepared in this example is 96.9%.

[0054] Example 7

[0055] In step 1), Zr / Ti=1.08, and the remaining steps are the same as those in Example 1. The relative density of the PZT ceramic prepared in this example is 95.4%.

[0056] Example 8

[0057] In step 1), Zr / Ti=1.08, and the other steps can be the same as in Example 2. The relative density of the PZT ceramic prepared in this example is 96.1%.

[0058] Example 9

[0059] In step 1), Zr / Ti=1.08, and the other steps can be the same as those in Example 3. The relative density of the PZT ceramic prepared in this example is 96.4%.

[0060] Example 10

[0061] In step 1), Zr / Ti=5.67, and the remaining steps can be the same as in Example 1. The relative density of the PZT ceramic prepared in this example is 95.2%.

[0062] Embodiment 11

[0063] In step 1), Zr / Ti=5.67, and the remaining steps can be the same as those in Example 2. The relative density of the PZT ceramic prepared in this example is 95.7%.

[0064] Example 12

[0065] In step 1), Zr / Ti=5.67, and the remaining steps can be the same as those in Example 3. The relative density of the PZT ceramic prepared in this example is 96%.

[0066] Embodiment 13

[0067] In step 1), Zr / Ti=19, and the other steps can be the same as in Example 1. The relative density of the PZT ceramic prepared in this example is 96.3%.

[0068] Embodiment 14

[0069] In step 1), Zr / Ti=19, and the other steps can be the same as those in Example 2. The relative density of the PZT ceramic prepared in this example is 96.2%.

[0070] Embodiment 15

[0071] In step 1), Zr / Ti=19, and the other steps can be the same as those in Example 3. The relative density of the PZT ceramic prepared in this example is 96.8%.

Claims

1. A method for preparing high-density PZT ceramics by slurry casting, Features: The specific method is as follows: 1) Pb 3 O 4 、ZrO 2 、TiO 2 The mixture was mixed evenly, and PZT ceramic materials with Zr / Ti=0.92, 1, 1.08, 5.67, and 19 were prepared respectively by solid phase method; 2) mixing the PZT ceramic material with deionized water and a dispersant, and ball-milling the mixture to obtain a slurry with a particle size of ≤200 µm; 3) Add a binder to the slurry, stir evenly, and inject it into a plaster mold at a pressure of 0.08-0.15 MPa. After molding, demould and dry to obtain a green body with a relative density greater than 50%; 4) placing the green body in a sintering furnace, heating it to 400-750°C at a rate of 0.5-1°C / min, and debinding for 4-6 hours; then heating it to 1200-1300°C at a rate of 3-5°C / min in an air atmosphere, burying it with lead and sintering it for 1-4 hours to obtain PZT ceramics.

2. The method for preparing high-density PZT ceramics by slip casting according to claim 1, Features: The amount of deionized water added is 20-30wt% of the total amount of the PZT ceramic material.

3. The method for preparing high-density PZT ceramics by slip casting according to claim 1, Features: The dispersant is ammonium polyacrylate, and the amount added is 0.5-1.5wt% of the total amount of the PZT ceramic material.

4. The method for preparing high-density PZT ceramics by slip casting according to claim 1, Features: The binder is polyvinyl alcohol, and its addition amount is 0.5-5wt% of the total amount of the PZT ceramic material.

5. The method for preparing high-density PZT ceramics by slip casting according to claim 1, Features: The rotation speed of the ball mill is 2000-2500 r / min; the ball milling medium is zirconia balls with a particle size of 0.3 mm.

6. The method for preparing high-density PZT ceramics by slip casting according to claim 1, Features: The drying method described in step 3) is: firstly place the demoulded green body in a room temperature environment of 20-30°C for drying for 3 days, and then transfer it to a 60°C oven for drying for 24 hours.

Citation Information

Patent Citations

  • High-density PZT (Pb-based lanthanum doped Zirconate Titanate) target and preparation method thereof

    CN107445617A