Piezoelectric ceramic with high piezoelectric constant and low strong field dielectric loss and preparation method thereof
Patent Information
- Application Number
- CN202411066701.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
[0003]一般而言,现有的P8压电陶瓷压电常数d33约240pC/N、强场介电损耗约tanδ≤0.8%@400V/mm,而P4和P5系列的强场损耗分别为1.5%和5%以上,P8系列强场损耗低的同时压电常数也会比较低,要达到一定的超声功率,产品体积就会较大
[0014] Compared with the existing technology, the piezoelectric ceramics provided by the present invention solve the problem of low piezoelectric constant (d) of the existing P8 series piezoelectric ceramic materials. 33 >300pC/N), and also has low strong field dielectric loss (tanδ≤0.75%@400V/mm), which can meet the needs of high-power transducers and reduce the size of the transducer. The method of the invention has the characteristics of simple process, no special equipment requirements, low cost, and is conducive to large-scale production, and can be used in components related to high-power ultrasonic transducers.
Smart Images

Figure CN118930261A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a piezoelectric ceramic with a high voltage constant and low strong field dielectric loss and a preparation method thereof. Background Art
[0002] The existing high-power piezoelectric ceramics are mainly P8 system, doped with calcium ferrite; they are mainly used in ultrasonic welding and ultrasonic flaw detection, but their piezoelectric constant is generally low, which limits their application range. With the development of electronic technology, piezoelectric transducers are required to be smaller and more powerful, so it is of great significance to develop piezoelectric ceramics with high piezoelectric constant and low dielectric loss in strong fields.
[0003] Generally speaking, the piezoelectric constant d of existing P8 piezoelectric ceramics is 33 About 240pC / N, strong field dielectric loss is about tanδ≤0.8%@400V / mm, while the strong field loss of P4 and P5 series are 1.5% and more than 5% respectively. The P8 series has low strong field loss and low piezoelectric constant. To achieve a certain ultrasonic power, the product volume will be larger. Therefore, it is of great significance to develop piezoelectric ceramic materials with high piezoelectric constant and low strong field dielectric loss. Summary of the invention
[0004] In view of the above-mentioned defects in the prior art, the present invention aims to provide a piezoelectric ceramic with high piezoelectric constant and low strong field dielectric loss. Another object of the present invention is to provide a method for preparing the piezoelectric ceramic.
[0005] In order to achieve the above-mentioned purpose, the piezoelectric ceramic structure provided by the present invention has the following general formula: Pb(Zr z Ti 1-z ) x (Co 1 / 3Nb 2 / 3 ) y (Mn 1 / 3 Nb 2 / 3 ) 1-x-y O3+nwt%A, x=0.85-0.95, y=0.01-0.06, z=0.45-0.55, n=0.1-1, A is the oxide of the modifying element, and the modifying element is one or more of Mg, Al, and Yb.
[0006] The preparation method provided by the present invention adopts the following technical scheme:
[0007] 1) According to the ratio in the general structural formula, Pb3O4, ZrO2, TiO2, Co2O3, Nb2O5, MnO2 and the modifying element oxide A are weighed in chemical proportion, ball-milled with deionized water, and dried to obtain a primary abrasive;
[0008] 2) placing the primary abrasive in a sintering furnace at 930-950° C. and calcining for 3 hours to obtain a pre-calcined material;
[0009] 3) ball-milling and drying the pre-sintered material again to obtain ceramic powder;
[0010] 4) uniformly mixing the ceramic powder and polyvinyl alcohol, granulating, and tableting to obtain a ceramic blank;
[0011] 5) placing the ceramic blank in a sintering furnace, heating it to remove the plastic, and then heating it to 1250-1280° C. and sintering it for 2-3 hours to obtain a ceramic sheet;
[0012] 6) printing silver paste on the front and back of the ceramic sheet, and then sintering it in a sintering furnace to obtain a silver-coated ceramic sheet;
[0013] 7) placing the silvered ceramic sheet in an environment with a temperature of 80-100° C. and an electric field strength of 3-4 kV / mm for a polarization time of 20-30 min.
[0014] Compared with the prior art, the piezoelectric ceramics provided by the present invention solve the problem of low piezoelectric constant of the existing P8 series piezoelectric ceramic materials (d 33 ﹥300pC / N), and at the same time has low strong field dielectric loss (tanδ≤0.75%@400V / mm), which can meet the use of high-power transducers and reduce the volume of the transducer. The method of the invention has the characteristics of simple process, no special equipment requirements, low cost, and is conducive to large-scale production, and can be used in high-power ultrasonic transducer related components. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is a scanning electron microscope image of a cross section of a piezoelectric ceramic provided by the present invention;
[0016] Figure 2 It is the XRD diffraction pattern of the pressed ceramic provided by the present invention;
[0017] Figure 3 It is the dielectric temperature spectrum of the piezoelectric ceramic provided by the present invention.
[0018] from Figure 1 It can be seen that the piezoelectric ceramic provided by the present invention has fine grains, good uniformity and consistency, and a dense structure, which provides a guarantee for the low loss of the ceramic.
[0019] from Figure 2 It can be seen that the piezoelectric ceramic provided by the present invention is a pure perovskite structure, which provides a guarantee for the stable performance of the product.
[0020] from Figure 3 It can be seen that the Curie temperature of the piezoelectric ceramic provided by the present invention is 328° C., which can meet the use requirements of high-power ceramics. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments:
[0022] Example 1
[0023] 1) According to the general structural formula Pb(Zr 0.51 Ti 0.49 ) 0.87 (Co 1 / 3 Nb 2 / 3 ) 0.04 (Mn 1 / 3 Nb 2 / 3 ) 0.09 O3+
[0024] In the ratio of 0.2wt% Al2O3, Pb3O4, ZrO2, TiO2, Co2O3, Nb2O5, MnO2 and Al2O3 are put into a mill, ball-milled with deionized water and dried to obtain primary abrasive;
[0025] 2) sieving the primary abrasive and pre-calcining it at 950° C. for 3 h to obtain a pre-calcined material;
[0026] 3) adding deionized water to the pre-sintered material, ball-milling and drying again to obtain ceramic powder;
[0027] 4) mixing the ceramic powder and polyvinyl alcohol uniformly, granulating, and pressing into tablets to obtain a ceramic blank; the amount of polyvinyl alcohol added is 5% of the weight of the ceramic powder;
[0028] 5) placing the ceramic blank in a sintering furnace, heating it to remove the plastic, and then heating it to 1260° C. and sintering it for 3 hours to obtain a ceramic sheet;
[0029] 6) printing silver paste on the front and back of the ceramic sheet, and then sintering it in a sintering furnace to obtain a silver-coated ceramic sheet;
[0030] 7) The silvered ceramic sheet was placed in an environment with a temperature of 90° C. and an electric field strength of 3.5 kv / mm for a polarization time of 30 min.
[0031] After aging for 24 hours, the comprehensive electrical properties of the above piezoelectric ceramics are: p =0.5,ε r =1100, tanδ=0.25%, tanδ=0.75%@400V / mm, d 33 =300pC / N.
[0032] Example 2
[0033] 1) According to the general structural formula Pb(Zr 0.51 Ti 0.49 )0.90 (Co 1 / 3 Nb 2 / 3 ) 0.06 (Mn 1 / 3 Nb 2 / 3 ) 0.04 O3+
[0034] In the ratio of 0.2wt% Al2O3+0.8wt% MgO, Pb3O4, ZrO2, TiO2, Co2O3, Nb2O5, MnO2, Al2O3 and MgO are put into a mill, ball-milled with deionized water and dried to obtain a primary abrasive;
[0035] 2) sieving the primary abrasive and pre-calcining it at 930° C. for 3 h to obtain a pre-calcined material;
[0036] 3) adding deionized water to the pre-sintered material, ball-milling and drying again to obtain ceramic powder;
[0037] 4) mixing the ceramic powder and polyvinyl alcohol uniformly, granulating, and pressing into tablets to obtain a ceramic blank; the amount of polyvinyl alcohol added is 5% of the weight of the ceramic powder;
[0038] 5) placing the ceramic blank in a sintering furnace, heating it to remove the plastic, and then heating it to 1250° C. and sintering it for 3 hours to obtain a ceramic sheet;
[0039] 6) printing silver paste on the front and back of the ceramic sheet, and then sintering it in a sintering furnace to obtain a silver-coated ceramic sheet;
[0040] 7) The silvered ceramic sheet was placed in an environment with a temperature of 90° C. and an electric field strength of 3.5 kv / mm for a polarization time of 30 min.
[0041] After aging for 24 hours, the comprehensive electrical properties of the above piezoelectric ceramics are: p =0.54,ε r =1300, tanδ=0.35%, tanδ=1.0%@400V / mm, d 33 =340pC / N.
[0042] Example 3
[0043] 1) According to the general structural formula Pb(Zr 0.51 Ti 0.49 ) 0.94 (Co 1 / 3 Nb 2 / 3 ) 0.04 (Mn 1 / 3 Nb 2 / 3 ) 0.02 O3+
[0044] In the ratio of 0.4wt% Al2O3+0.6wt% Yb2O3, Pb3O4, ZrO2, TiO2, Co2O3, Nb2O5, MnO2, Al2O3 and Yb2O3 are put into a mill, ball-milled with deionized water, and dried to obtain a primary abrasive;
[0045] 2) sieving the primary abrasive and pre-calcining it at 930° C. for 3 h to obtain a pre-calcined material;
[0046] 3) adding deionized water to the pre-sintered material, ball-milling and drying again to obtain ceramic powder;
[0047] 4) mixing the ceramic powder and polyvinyl alcohol uniformly, granulating, and pressing into tablets to obtain a ceramic blank; the amount of polyvinyl alcohol added is 5% of the weight of the ceramic powder;
[0048] 5) placing the ceramic blank in a sintering furnace, heating it to remove the plastic, and then heating it to 1280° C. and sintering it for 3 hours to obtain a ceramic sheet;
[0049] 6) printing silver paste on the front and back of the ceramic sheet, and then sintering it in a sintering furnace to obtain a silver-coated ceramic sheet;
[0050] 7) The silvered ceramic sheet was placed in an environment with a temperature of 90° C. and an electric field strength of 3.5 kv / mm for a polarization time of 30 min.
[0051] After aging for 24 hours, the comprehensive electrical properties of the above piezoelectric ceramics are: p =0.60,ε r =1600, tanδ=0.41%, tanδ=1.2%@400V / mm, d 33 =360pC / N.
[0052] The electrical performance parameters of the piezoelectric ceramics prepared in the above embodiments are as follows:
[0053] Table 1: Example ceramic parameters
[0054]
Claims
1. A piezoelectric ceramic with high piezoelectric constant and low dielectric loss in strong field, characterized in that The general structural formula of the piezoelectric ceramic is: Pb(Zr z Ti 1-z ) x (Co 1 / 3 Nb 2 / 3 ) y (Mn 1 / 3 Nb 2 / 3 ) 1-x-y O3+nwt%A, x=0.85-0.95, y=0.01-0.06, z=0.45-0.55, n=0.1-1, A is the oxide of the modifying element, and the modifying element is one or more of Mg, Al, and Yb.
2. A method for preparing the piezoelectric ceramic with high piezoelectric constant and low dielectric loss in strong field according to claim 1, characterized in that Here are the steps: 1) According to the ratio in the general structural formula, Pb3O4, ZrO2, TiO2, Co2O3, Nb2O5, MnO2 and the modifying element oxide A are weighed in chemical proportion, ball-milled with deionized water, and dried to obtain a primary abrasive; 2) placing the primary abrasive in a sintering furnace at 930-950° C. and calcining for 3 hours to obtain a pre-calcined material; 3) ball-milling and drying the pre-sintered material again to obtain ceramic powder; 4) uniformly mixing the ceramic powder and polyvinyl alcohol, granulating, and tableting to obtain a ceramic blank; 5) placing the ceramic blank in a sintering furnace, heating it to remove the plastic, and then heating it to 1250-1280° C. and sintering it for 2-3 hours to obtain a ceramic sheet; 6) printing silver paste on the front and back of the ceramic sheet, and then sintering it in a sintering furnace to obtain a silver-coated ceramic sheet; 7) placing the silvered ceramic sheet in an environment with a temperature of 80-100° C. and an electric field strength of 3-4 kV / mm for a polarization time of 20-30 min.
Citation Information
Patent Citations
Piezoelectric ceramic composition and resonator
CN101148350A
Lead manganate niobate-lead nickelate niobate-lead zirconate titanate high-voltage ferroelectric ceramic with ultralow dielectric loss and preparation method thereof
CN113185289A
Al2o3-doped pmn-PZT piezoelectric ceramics and method for producing the same
KR100663972B1
A piezo ceramic composition
KR1020040049383A