Bismuth calcium niobate-based textured ceramic material and preparation method thereof
Through the preparation method of bismuth calcium niobate-based textured ceramic material, the doping and casting forming process are used to solve the problem of insufficient performance of high-temperature piezoelectric ceramics in high-temperature environments, and the high-voltage electrical performance and high Curie temperature ceramics are realized Materials, suitable for industrial production.
Patent Information
- Application Number
- CN202411077319.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
The existing high-temperature piezoelectric ceramics cannot operate stably in a high temperature environment above 500°C, and the piezoelectric properties of bismuth layered structure piezoelectric ceramics are limited and difficult to optimize through manual polarization.
The preparation method of bismuth calcium niobate-based textured ceramic material is adopted. By mixing bismuth calcium niobate ceramic powder and template grains, combined with casting and sintering processes, the scraper height and sintering temperature are controlled to achieve the grain height orientation. 排列,提高压电性能。
The piezoelectric properties and Curie temperature of bismuth niobate-based textured ceramic materials were significantly improved, with the piezoelectric coefficient reaching 27.2pC/N and the Curie temperature reaching 949.4℃, and the structural stability of the material was maintained.
Smart Images

Figure CN118930263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic material preparation, and specifically relates to a bismuth calcium niobate-based textured ceramic material and a preparation method thereof. Background Art
[0002] High-temperature piezoelectric ceramics, as a type of piezoelectric ceramics that can work in high-temperature environments, are widely used in sensors, filters, transducers, etc. At present, due to the limitation of the Curie temperature of piezoelectric ceramics, the operating temperature of most high-temperature piezoelectric devices is below 500°C.
[0003] However, in some special high-temperature fields, such as aerospace, nuclear industry, and oil exploration, there is an urgent need for piezoelectric devices that can work stably in high-temperature environments above 500°C. The Curie temperatures of the currently commercialized PZT (PbZrO3-PbTiO3) and PT (PbTiO3) systems are both below 490°C. When the Curie temperature is higher, depolarization will occur and the device cannot be used. Therefore, there is an urgent need to develop a piezoelectric ceramic with an ultra-high Curie temperature for use in some special high-temperature environments.
[0004] Bismuth layered piezoelectric ceramics have the characteristics of high Curie temperature (650-950℃), low dielectric constant, low aging rate and high resistivity. This makes bismuth layered piezoelectric ceramics have broad prospects in the manufacture of high-temperature piezoelectric sensors. Bismuth layered piezoelectric ceramics are composed of bismuth oxide layers ((Bi2O2) 2+ ) and perovskite-like layers are alternately stacked, and its general chemical formula is (Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- , where A represents a twelve-coordinated monovalent, divalent, or trivalent cation or a combination thereof, forming a dodecahedral coordination; B represents a series of transition metal cations that satisfy six-coordinate coordination, forming an octahedral coordination; m represents the number of oxygen octahedral layers in the perovskite-like structure, and the value range is 1 to 6. Among them, calcium bismuth niobate (CaBi2Nb2O9, m=2) is a typical bismuth layered structure piezoelectric ceramic, and its Curie temperature can reach 950°C, which is one of the bismuth layered structure piezoelectric ceramics with the highest Curie temperature. However, due to its special two-dimensional structure, the spontaneous polarization is confined to the ab plane, which makes it have a high coercive field and an extremely low piezoelectric coefficient (5 to 7pC / N). It is difficult to obtain a ceramic body with excellent piezoelectric properties through artificial polarization, which is also a common problem of bismuth layered structure ferroelectrics. At present, the modification method of CBN ceramics is mainly ion doping, but the piezoelectric performance of the modified CBN ceramics is limited (d 33 <20pC / N), and the Curie temperature decreases after doping. Summary of the invention
[0005] In view of the deficiencies in the prior art, the first object of the present invention is to provide a method for preparing a calcium bismuth niobate-based textured ceramic material. The preparation method provided by the present invention is simple and controllable and suitable for industrial production.
[0006] The second object of the present invention is to provide a bismuth calcium niobate-based textured ceramic material prepared by the above-mentioned preparation method, wherein the bismuth calcium niobate-based textured ceramic material has highly oriented grains, and the high orientation of the grains is conducive to greatly improving its residual polarization strength, thereby improving the piezoelectric performance.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme:
[0008] The invention discloses a method for preparing a bismuth calcium niobate-based textured ceramic material, comprising the steps of mixing doped bismuth calcium niobate ceramic powder, doped bismuth calcium niobate ceramic template grains, a solvent, a dispersant, a plasticizer, and a binder to obtain a ceramic slurry, performing tape casting on the ceramic slurry on a tape casting machine to obtain a diaphragm, stacking the diaphragms to obtain a green body, sequentially subjecting the green body to a first pressing molding, debinding, and a second pressing molding to obtain a compact, and then sintering the compact to obtain the bismuth calcium niobate-based textured ceramic material;
[0009] The chemical formula of the doped calcium bismuth niobate ceramic powder is Ca 0.95 Na 0.025 Sm 0.025 Bi2Nb2O9;
[0010] The doped calcium bismuth niobate ceramic template grains are in the form of flakes, and the chemical formula is: Ca 0.95 Na 0.025 Sm 0.025 Bi2Nb2O9;
[0011] During the tape casting, the scraper height is first set to 25-200 μm, and the first tape casting is performed. After the tape casting is completed, the film is dried to obtain a first layer of ceramic green film; then the scraper height is set to be 25-200 μm higher than the first layer of ceramic green film, preferably 25-50 μm, and the second tape casting is performed. After the tape casting is completed, the film is dried to obtain a second layer of ceramic green film; the above operation is repeated to obtain the nth layer of ceramic green film, where n is 5 to 20, i.e., a diaphragm.
[0012] The preparation method of the present invention uses the same flake doped calcium bismuth niobate ceramic powder as the template and the same composition as the doped calcium bismuth niobate ceramic powder, which can avoid the internal stress caused by the different lattice constants between the original seed crystal part and the part formed by swallowing the matrix particles after the seed crystal engulfs the matrix particles, thereby avoiding the influence of the internal stress on the piezoelectric performance. During the tape casting, the scraper can be lowered to a very small height (25μm) through the process of tape casting-drying-re-casting, so that the seed crystal can be highly oriented and arranged, and the texture degree is higher.
[0013] In the present invention, the scraper height needs to be controlled. If it is too low, the degree of seed crystal orientation will be higher, but the degree is limited and the scraping efficiency is not high. If it is too high, the degree of seed crystal orientation will be reduced, the texture of the ceramic will be reduced, and the piezoelectric performance will deteriorate.
[0014] According to a preferred embodiment, the preparation process of the doped calcium bismuth niobate ceramic powder is as follows: CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder are prepared in a designed proportion to obtain a mixed powder, and the mixed powder is subjected to a first ball milling, pre-sintering and a second ball milling.
[0015] Further preferably, the first ball milling is wet ball milling, the ball milling medium is anhydrous ethanol, the ball milling time is 8-24 hours, and the ball milling speed is 200-400 r / min.
[0016] Further preferably, the pre-sintering temperature is 900-1000° C., and the pre-sintering time is 2-6 hours.
[0017] Further preferably, the second ball milling is wet ball milling, the ball milling medium is anhydrous ethanol, the ball milling time is 8-24h, and the ball milling speed is 200-400r / min.
[0018] The ball milled material obtained after the second ball milling is dried and ground to obtain a mixed powder.
[0019] In a preferred embodiment, the preparation process of the doped calcium bismuth niobate ceramic template grains is as follows: CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder are mixed to obtain a mixture, the mixture is ball-milled with neutral salt to obtain ball-milled powder, the ball-milled powder is sintered to obtain sintered powder, and then washed to obtain doped calcium bismuth niobate ceramic template grains.
[0020] Further preferably, the neutral salt consists of NaCl and KCl; in the neutral salt, the molar ratio of NaCl:KCl is 0.5 to 2:1.
[0021] Further preferably, the mass ratio of the mixture to the neutral salt is 0.5 to 2:1.
[0022] Further preferably, the ball milling is wet ball milling, the ball milling medium is anhydrous ethanol, the material of the grinding balls is zirconium oxide, wherein the mass ratio of the total mass of the mixture and the neutral salt to the mass of the grinding balls and the ball milling medium is 1:1-1.5:0.5-0.65, the rotation speed of the ball mill is 200-400r / min, and the ball milling time is 8-48h.
[0023] In the actual operation process, the material obtained after ball milling is dried and sieved.
[0024] Further preferably, the sintering temperature is 9500-1100° C., the sintering time is 6-24 h, and the heating rate is 5° C. / min.
[0025] Further preferably, the sintered powder is cleaned until the conductivity drops to 3 μS / cm.
[0026] In a preferred embodiment, in the ceramic slurry, the amount of the ceramic template grains doped with bismuth calcium niobate is 5-20% of the mass of the ceramic powder doped with bismuth calcium niobate, preferably 10-20%, preferably 10-15%. The inventors have found that by controlling the amount of the ceramic template grains doped with bismuth calcium niobate within the above range, the higher the texture of the ceramic, the better the piezoelectric properties of the ceramic material finally obtained.
[0027] The preferred scheme is that the process of mixing to obtain ceramic slurry is: adding doped calcium bismuth niobate ceramic powder to a solvent and a dispersant and ball milling for 12-48 hours to obtain a mixed solution, adding a plasticizer and a binder to the mixed solution and ball milling for 12-48 hours to obtain a mixed viscous solution, and then adding doped calcium bismuth niobate ceramic template grains to the mixed viscous solution and ball milling for 0.5-12 hours to obtain a ceramic slurry.
[0028] The inventors have found that by adopting the slurry system of the present invention, in conjunction with the slurry preparation process provided in the invention, the resulting slurry has a good casting effect, so that the performance of the final textured ceramic is optimized.
[0029] In the actual operation process, first, the prepared slurry is placed in a vacuum environment and slowly stirred to remove the bubbles in the slurry; then the treated ceramic slurry is poured into the casting machine, the scraper height is set in turn, and the casting process is carried out. After the casting process is completed, the ceramic membrane is cut to obtain a membrane sheet.
[0030] In a preferred embodiment, the solvent is a mixed solution of xylene and anhydrous ethanol, wherein the volume ratio of xylene to anhydrous ethanol is 1-3:1.
[0031] In a preferred embodiment, the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to the solvent is 50g:30-50ml.
[0032] In a preferred embodiment, the dispersant is triethyl phosphate, and the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to the dispersant is 50g:0.1-0.5ml.
[0033] In a preferred embodiment, the plasticizer is composed of polyethylene glycol and dibutyl phthalate, the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to polyethylene glycol is 50g:4-10ml, and the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to dibutyl phthalate is 50g:0-6ml.
[0034] In a preferred embodiment, the binder is polyvinyl butyral, and the mass ratio of the doped calcium bismuth niobate ceramic powder to polyvinyl butyral is 50:1-6.
[0035] In a preferred solution, the membrane sheets are stacked and then vacuum dried to obtain a green body, the drying temperature is controlled to be 30-100° C., and the internal pressure is controlled to be 20-70 kPa. The bubbles in the green body are discharged by vacuum drying.
[0036] In a preferred embodiment, the pressure of the first pressing is 100-500 MPa, and the time of the first pressing is 10-30 min. In the actual operation, the green body is placed in a cold isostatic press and pressed to make the green body dense.
[0037] In a preferred embodiment, the debinding process is as follows: heating the temperature from room temperature to 150-200°C at a rate of 0.5-3°C / min and keeping the temperature for 2-6h, and then heating the temperature to 500-600°C at a rate of 0.1-1°C / min and keeping the temperature for 6-12h.
[0038] In a preferred embodiment, the pressure of the second pressing and molding is 100-500 MPa, and the time of the second pressing and molding is 10-30 min.
[0039] The inventors have found that by controlling the pressing pressure within the range of the present invention and applying the same pressure again for pressing after debinding, the density of the material can be further improved, so that the density of the final textured ceramic is the highest.
[0040] In a preferred embodiment, the sintering process is as follows: heating the compact from room temperature to 1100-1200° C. at a heating rate of 1-10° C. / min and maintaining the temperature for 18-24 hours.
[0041] The sintering process of the present invention ensures the high orientation arrangement of grains and improves the texture degree through long-term sintering and heat preservation.
[0042] The present invention also provides a bismuth calcium niobate-based textured ceramic material prepared by the above preparation method.
[0043] Beneficial Effects
[0044] The preparation method of the present invention uses the same flake doped bismuth calcium niobate ceramic powder as the template and the same composition as the doped bismuth calcium niobate ceramic powder, which can avoid the internal stress caused by the different lattice constants between the original seed crystal part and the part formed by swallowing the matrix after the seed crystal engulfs the matrix particles, thereby avoiding the influence of the internal stress on the piezoelectric performance. During the tape casting, the scraper can be lowered to a very small height (25μm) through the process of tape casting-drying-re-casting, so that the seed crystal can be highly oriented. In addition, during the sintering process of the present invention, the sintering temperature is controlled to be long enough. Finally, all the grains are oriented because the oriented seed crystal engulfs the randomly oriented matrix particles during the sintering process to form a large grain with the same orientation as the seed crystal. Only when the sintering process is guaranteed to be long enough can the seed crystal completely engulf the randomly oriented matrix particles, thereby ensuring the high orientation of the grains. Under the above synergy, the bismuth calcium niobate-based textured ceramic material of the present invention has excellent piezoelectric properties.
[0045] In addition, in the present invention, since only the orientation and size of the grains are changed, the composition of the material does not change, that is, the degree of lattice distortion, electronegativity and other factors of the material are not changed, and the stability of the structure is not greatly affected, thereby avoiding affecting the Curie temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 Schematic diagram of the tape casting process in the present invention.
[0047] Figure 2 SEM image of the ceramic obtained in Example 1.
[0048] Figure 3 Dielectric temperature spectrum of the ceramic obtained in Example 1 and its corresponding Curie temperature T c、
[0049] Figure 4 PE hysteresis loop of the ceramic obtained in Example 1.
[0050] Figure 5 SEM image of the ceramic obtained in Example 2.
[0051] Figure 6 Dielectric temperature spectrum of the ceramic obtained in Example 2 and its corresponding Curie temperature T c、
[0052] Figure 7 PE hysteresis loop of the ceramic obtained in Example 2.
[0053] Figure 8 SEM image of the ceramic obtained in Example 3.
[0054] Fig. 9 Dielectric temperature spectrum of the ceramic obtained in Example 3 and its corresponding Curie temperature Tc、
[0055] Fig.10 PE hysteresis loop of the ceramic obtained in Example 3.
[0056] Fig.11 SEM image of the ceramic obtained in Example 4.
[0057] Fig.12 Dielectric temperature spectrum of the ceramic obtained in Example 4 and its corresponding Curie temperature T c、
[0058] Fig.13 PE hysteresis loop of the ceramic obtained in Example 4.
[0059] Fig.14 SEM image of the ceramic obtained in Comparative Example 1.
[0060] Fig.15 Dielectric temperature spectrum of the ceramic obtained in Comparative Example 1 and its corresponding Curie temperature T c、
[0061] Fig.16 PE hysteresis loop of the ceramic obtained in Comparative Example 1.
[0062] Fig.17 XRD patterns of the ceramics obtained in Examples 1-4 and Comparative Example 1 and their corresponding textures.
[0063] Fig.18 Piezoelectric coefficient d of the ceramics obtained in Examples 1-4 and Comparative Example 1 33 .
[0064] Fig.19 SEM image of the ceramic obtained in Comparative Example 3. DETAILED DESCRIPTION
[0065] Embodiment 1:
[0066] 1. Ca 0.95 Na 0.025 Sm 0.025 Preparation of Bi2Nb2O9 template grains:
[0067] The raw materials of calcium bismuth niobate doped with CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder were weighed according to the stoichiometric ratio, and the neutral salt NaCl-KCl (the molar ratio of NaCl to KCl was 1:1) was selected, and the mass ratio of the raw materials to the neutral salt was 1:1;
[0068] The raw materials, neutral salt, zirconium balls and anhydrous ethanol were placed in a ball mill at a mass ratio of 1:1.5:0.65 and ball-milled at a speed of 300 r / min for 24 hours, and then dried and sieved; the dried powder was poured into a crucible and kept at a temperature of 1050°C for 6 hours with a heating rate of 5°C / min; the synthesized sample was washed with deionized water until the conductivity of the washed water dropped to 3μS / cm to obtain the desired powder.
[0069] 2. Ca 0.95 Na 0.025 Sm 0.025 Preparation of Bi2Nb2O9 ceramic matrix powder:
[0070] Preparation of the chemical formula Ca 1-2x Sm x Na x Bi2Nb2O9, and Sm and Na doped modified calcium bismuth niobate ceramics when x=0.025, referred to as CBNNS-0.025.
[0071] Analytically pure powder raw materials CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder were weighed according to the stoichiometric ratio and prepared according to the traditional solid phase preparation process. The raw materials were then mixed with anhydrous ethanol, ball-milled at 300 r / min for 8 hours, pre-calcined at 925°C for 2 hours, ball-milled for a second time at 300 r / min for 12 hours, and dried to obtain the ceramic matrix powder.
[0072] 3. Prepare slurry
[0073] The composition of the ceramic slurry is shown in Table 1. First, weigh an appropriate amount of ceramic matrix powder (composition: CBNNS-0.025), add an appropriate amount of xylene / anhydrous ethanol as a solvent and triethyl phosphate as a dispersant, and ball mill for 24 hours. After ball milling, add plasticizer (polyethylene glycol and dibutyl phthalate) and binder (polyvinyl butyral), continue ball milling for 24 hours, and then add 5wt% of the ceramic matrix powder mass template grains and ball mill for 0.5 hours.
[0074] Table 1 Composition of tape casting slurry
[0075]
[0076] 4. Tape casting
[0077] The tape casting process is shown in the figure. First, the prepared slurry is placed in a vacuum environment and slowly stirred to remove the bubbles in the slurry; then the treated ceramic slurry is poured into the tape casting machine, the scraper height is set to 25μm, and the tape casting operation is performed. After the tape casting is completed, it is dried to obtain the first layer of ceramic green film. Then the scraper height is set to 50μm, and the tape casting operation is performed on the first layer of ceramic green film, and the second layer of ceramic green film is dried. The scraper height is set to 75, 100, 125, and 200μm respectively, and the above operations are repeated to obtain the final ceramic film.
[0078] 5. Cutting and stacking
[0079] The scraped ceramic membrane was cut into 30×30 mm squares and stacked to a height of 20 mm. The stacked green pieces were then placed in a vacuum drying oven for vacuum drying. The temperature was set to 100°C and the internal air pressure was set to 20 kPa to expel the bubbles in the green pieces.
[0080] 6. Debinding and densification
[0081] The green body is placed in a cold isostatic press, and the pressure is set to 500MPa for 30 minutes to further densify the green body. Then it is placed in a muffle furnace for debinding. The debinding process is: 1℃ / min from room temperature to 180℃ for 6 hours, then 0.2℃ / min to 600℃ for 12 hours. After debinding, cold isostatic pressing is performed at the same pressure for 30 minutes.
[0082] 7. Sintering
[0083] The densified ceramic green body was placed in a muffle furnace and heated from room temperature to 1150°C at a rate of 5°C / min for 18 h to obtain textured CBNNS-0.025 ceramics.
[0084] Its texture degree f reaches 85.6%, and the residual polarization P r 20.36μC / cm 2 , piezoelectric coefficient d 33 It reached 27.2pC / N and the Curie temperature was 949.4℃.
[0085] Embodiment 2:
[0086] The other conditions are the same as those in Example 1, except that the template grain content is 10 wt % to obtain the textured CBNNS-0.025 ceramic, whose texture degree f reaches 95.2% and the residual polarization P r 25.78μC / cm 2 , piezoelectric coefficient d 33 It reached 31.1pC / N and the Curie temperature was 950.7℃.
[0087] Embodiment 3:
[0088] The other conditions are the same as those in Example 1, except that the template grain content is 15 wt % to obtain the textured CBNNS-0.025 ceramic, whose texture degree f reaches 97.9% and the residual polarization P r 26.81μC / cm 2 , piezoelectric coefficient d 33 It reached 30.8pC / N and the Curie temperature was 946.8℃.
[0089] Embodiment 4:
[0090] The other conditions are the same as those in Example 1, except that the template grain content is 20 wt % to obtain the textured CBNNS-0.025 ceramic, whose texture degree f reaches 98% and the residual polarization P r 26.83μC / cm 2 , piezoelectric coefficient d 33 It reached 30.4pC / N and the Curie temperature was 949.6℃.
[0091] Comparative Example 1:
[0092] The other conditions are the same as those in Example 1, except that the template grain content is 0 wt % to obtain the textured CBNNS-0.025 ceramic, whose texture degree f reaches 37.2% and the residual polarization P r 11.84μC / cm 2 , piezoelectric coefficient d 33 It reached 12.8pC / N and the Curie temperature was 946.1℃.
[0093] Comparative Example 2
[0094] The other conditions were the same as those in Example 1. The template was changed to pure CBN seed crystal. CBNNS-0.25 textured ceramics were prepared using 10 wt % of the content. The texture degree was 92%. The piezoelectric performance was d 33 It is 20.5pC / N.
[0095] Comparative Example 3
[0096] The other conditions were the same as those in Example 1. A single scraper height of 200 μm and a seed crystal content of 5 wt% were used to prepare CBNNS-0.025 textured ceramics. The grain orientation was significantly worse than that of the textured ceramics with 25 μm and 5 wt% seed crystal content. The texture degree was 46.52%, and the piezoelectric performance was d 33 It is 15pC / N.
Claims
1. A method for preparing a calcium bismuth niobate-based textured ceramic material, characterized in that: A ceramic slurry is obtained by mixing a bismuth calcium niobate-doped ceramic powder, a bismuth calcium niobate-doped ceramic template grain, a solvent, a dispersant, a plasticizer, and a binder, and the ceramic slurry is tape-cast on a tape-casting machine to obtain a diaphragm, and the diaphragms are stacked to obtain a green body, and the green body is sequentially subjected to a first pressing molding, a binder removal, and a second pressing molding to obtain a compact, and the compact is sintered to obtain a bismuth calcium niobate-based textured ceramic material; The chemical formula of the doped calcium bismuth niobate ceramic powder is Ca 0.95 Na 0.025 Sm 0.025 Bi2Nb2O9; The doped calcium bismuth niobate ceramic template grains are in the form of flakes, and the chemical formula is: Ca 0.95 Na 0.025 Sm 0.025 Bi2Nb2O9; During the tape casting, the scraper height is first set to 25-200 μm, and the first tape casting is performed. After the tape casting is completed, the film is dried to obtain a first layer of ceramic green film; then the scraper height is set to be 25-200 μm higher than the first layer of ceramic green film, and the second tape casting is performed. After the tape casting is completed, the film is dried to obtain a second layer of ceramic green film; the above operation is repeated to obtain the nth layer of ceramic green film, where n is 5 to 20, i.e., a diaphragm.
2. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The preparation process of the doped calcium bismuth niobate ceramic powder is as follows: CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder are prepared according to the designed proportion to obtain a mixed powder, and the mixed powder is subjected to a first ball milling, pre-sintering and a second ball milling to obtain the obtained powder; The first ball milling is wet ball milling, the ball milling medium is anhydrous ethanol, the ball milling time is 8-24h, and the ball milling speed is 200-400r / min; The pre-sintering temperature is 900-1000°C, and the pre-sintering time is 2-6h; The second ball milling is wet ball milling, the ball milling medium is anhydrous ethanol, the ball milling time is 8-24h, and the ball milling speed is 200-400r / min; The ball milled material obtained after the second ball milling is dried and ground to obtain a mixed powder.
3. The method for preparing a calcium bismuth niobate-based textured ceramic material according to claim 1, characterized in that: The preparation process of the doped calcium bismuth niobate ceramic template grains is as follows: CaCO3 powder, Na2CO3 powder, Sm2O3 powder, Bi2O3 powder and Nb2O5 powder are mixed to obtain a mixture, the mixture is ball-milled with neutral salt to obtain ball-milled powder, the ball-milled powder is sintered to obtain sintered powder, and then the doped calcium bismuth niobate ceramic template grains are obtained by washing; The neutral salt is composed of NaCl and KCl; in the neutral salt, in terms of molar ratio, NaCl:KCl=0.5:~2:1; The mass ratio of the mixture to the neutral salt is 0.5-2:1; The ball mill is a wet ball mill, the ball milling medium is anhydrous ethanol, the material of the grinding ball is zirconium oxide, wherein the total mass ratio of the mixture and the neutral salt to the grinding ball and the ball milling medium is 1:1-1.5:0.5-0.65, the rotation speed of the ball mill is 200-400r / min, and the ball milling time is 8-48h; The sintering temperature is 9500-1100°C, the sintering time is 6-24h, and the heating rate is 5°C / min; The sintered powder is cleaned until the conductivity drops to 3 μS / cm or less.
4. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: In the ceramic slurry, the added amount of the doped calcium bismuth niobate ceramic template grains is 5-20% of the mass of the doped calcium bismuth niobate ceramic powder.
5. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The process of mixing to obtain ceramic slurry is as follows: adding doped calcium bismuth niobate ceramic powder to a solvent and a dispersant and ball-milling for 12-48 hours to obtain a mixed solution, adding a plasticizer and a binder to the mixed solution and ball-milling for 12-48 hours to obtain a mixed viscous solution, and then adding doped calcium bismuth niobate ceramic template grains to the mixed viscous solution and ball-milling for 0.5-12 hours to obtain a ceramic slurry.
6. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The solvent is a mixed solution of xylene and anhydrous ethanol, wherein the volume ratio of xylene to anhydrous ethanol is 1-3:1; The solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to the solvent is 50g:30-50ml; The dispersant is triethyl phosphate, and the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to the dispersant is 50g:0.1-0.5ml; The plasticizer is composed of polyethylene glycol and dibutyl phthalate, the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to the polyethylene glycol is 50g:4-10ml, and the solid-liquid mass volume ratio of the doped calcium bismuth niobate ceramic powder to dibutyl phthalate is 50g:0-6ml; The binder is polyvinyl butyral, and the mass ratio of the doped calcium bismuth niobate ceramic powder to polyvinyl butyral is 50:1-6.
7. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The membrane sheets are stacked and then vacuum dried to obtain a green body, and the drying temperature is controlled to be 30-100° C. and the internal pressure is controlled to be 20-70 kPa.
8. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The pressure of the first pressing and molding is 100-500MPa, and the time of the first pressing and molding is 10-30min; The debinding process is as follows: heating from room temperature to 150-200°C at a rate of 0.5-3°C / min and keeping the temperature for 2-6h, then heating to 500-600°C at a rate of 0.1-1°C / min and keeping the temperature for 6-12h; The pressure of the second pressing and molding is 100-500 MPa, and the time of the second pressing and molding is 10-30 min.
9. The method for preparing a bismuth calcium niobate-based textured ceramic material according to claim 1, characterized in that: The sintering process is: heating the compact from room temperature to 1100-1200° C. at a heating rate of 1-10° C. / min and keeping the temperature for 18-24 hours.
10. Calcium bismuth niobate-based textured ceramic material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Textured calcium bismuth niobate ceramic material and preparation method thereof
CN101973764A
Sodium bismuth titanate-barium titanate-potassium bismuth titanate lead-free piezoelectric texture ceramic and preparation method thereof
CN103613382A
Preparation method of barium calcium zirconate titanate lead-free piezoelectric textured ceramic
CN105418067A
Electronic product shell, preparation method of electronic product shell and rear covers of mobile phones
CN110862260A
Doped and modified bismuth calcium niobate-based ceramic material and preparation method thereof
CN114507070A
Cited By
Bismuth calcium niobate textured ceramic and preparation method thereof
CN121974690A