KNN-based leadless piezoelectric ceramic and preparation method thereof

By doping Ta and (Li1-zAgz)SbO3 in KNN ceramics, combining rare earth and trivalent metal elements, the piezoelectric properties of KNN ceramics are improved, and the problems of lead-based ceramic pollution and insufficient performance of pure KNN ceramics are solved, and the results are achieved. Development of high-performance lead-free piezoelectric ceramics.

CN118930264AInactive Publication Date: 2024-11-12HUNAN CHENGXIANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095643.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lead-based piezoelectric ceramic materials are difficult to obtain practical application because they contain lead and pollute the environment and are harmful to health, and the piezoelectric coefficient d33 of pure KNN ceramics is low.

Method used

KNN-based lead-free piezoelectric ceramics with chemical structural formula (1-α-β)(K1-xNax)(Nb1-yTay)O3-α(Li1-zAgz)SbO3-βNMO3 are used, and are doped by Ta, (Li1-zAgz ) SbO3 flux is doped with rare earth and trivalent metal elements, adjusting the phase structure and sintering characteristics, and improving piezoelectric properties.

Benefits of technology

The piezoelectric performance improvement of KNN ceramics has been achieved, and d33 reaches 400pC/N, which is far higher than pure KNN ceramics, and has better practical application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930264A_ABST
    Figure CN118930264A_ABST
Patent Text Reader

Abstract

The invention relates to the field of piezoelectric ceramic materials, in particular to KNN-based leadless piezoelectric ceramic and a preparation method thereof, the chemical structural formula of the KNN-based leadless piezoelectric ceramic is as follows: (1-alpha-beta) (K1-xNax) (Nb1-yTay) O3-alpha (Li1-zAgz) SbO3-beta NMO3, wherein x is greater than or equal to 0.3 and less than or equal to 0.6, y is greater than 0 and less than or equal to 0.3, and z is greater than 0 and less than or equal to 0.3; 0 < alpha < = 0.1, 0 < beta < = 0.1; n is a rare earth element; m is a trivalent metal element, the prepared KNN-based leadless piezoelectric ceramic has excellent piezoelectric performance, d33 reaches 400 pC / N and is far higher than that of pure KNN ceramic, and the KNN-based leadless piezoelectric ceramic has better practical application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of piezoelectric ceramic materials, in particular to a KNN-based lead-free piezoelectric ceramic and a preparation method thereof. Background Art

[0002] Piezoelectric materials have been widely used in transducers, ultrasonic motors, printers, actuators and high-precision positioning systems due to their ability to directly convert mechanical energy into electrical energy. In the past few decades, the lead zirconate titanate (PZT) family has dominated the global piezoelectric ceramic market with its excellent piezoelectric properties. However, since PZT-based piezoelectric ceramics contain a lot of lead elements, they not only pollute the environment, but also endanger human health. Therefore, the development of high-performance lead-free piezoelectric ceramics is urgent.

[0003] In the past few decades, potassium sodium niobate (KNN)-based lead-free piezoelectric ceramics have attracted the attention of researchers due to their high Curie temperature and relatively excellent piezoelectric properties. Although KNN-based piezoelectric materials may be used in aerospace and electronic information fields, it should be noted that the piezoelectric coefficient d of pure KNN ceramics is 33 It is only 80pC / N, which is far behind PZT-based piezoelectric ceramics and is difficult to be used in practice. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a KNN-based lead-free piezoelectric ceramic and a preparation method thereof.

[0005] The technical solutions adopted are as follows:

[0006] A KNN-based lead-free piezoelectric ceramic, the chemical structure of which is shown below:

[0007] (1-α-β)(K 1-x Na x )(Nb 1-y Ta y )O3-α(Li 1-z Ag z )SbO3-βNMO3

[0008] Among them, 0.3≤x≤0.6, 0<y≤0.3, 0<z≤0.3;

[0009] 0<α≤0.1, 0<β≤0.1;

[0010] N is a rare earth element;

[0011] M is a trivalent metal element.

[0012] Further, 0.45≤x≤0.55, 0.1≤y≤0.2, 0.05≤z≤0.15.

[0013] Further, x=0.5, y=0.15, z=0.1.

[0014] Furthermore, 0.03≤α≤0.06, 0.03≤β≤0.06.

[0015] Further, α=0.05, β=0.05.

[0016] Furthermore, N is La.

[0017] Furthermore, M is Al, Fe or Co.

[0018] The present invention also provides a method for preparing a KNN-based lead-free piezoelectric ceramic:

[0019] According to the stoichiometric 1-x Na x )(Nb 1-y Ta y )O3、(Li 1-z Ag z )SbO3 and NMO3 are mixed and ball-milled and then dried to obtain a mixed powder, the mixed powder is granulated, sieved, and pressed into a green body, and the green body is heated to remove binder and then sintered.

[0020] Furthermore, the debinding temperature is 650-750°C, and the debinding time is 1-5h.

[0021] Furthermore, the sintering temperature is 1050-1150° C., and the sintering time is 1-5 h.

[0022] Beneficial effects of the present invention:

[0023] The present invention provides a KNN-based lead-free piezoelectric ceramic, wherein Ta and Nb are elements of the same subgroup, have the same valence and almost the same atomic radius, and Ta replaces the position of Nb at the B position in the KNN ceramic, thereby affecting the physical structure of the KNN piezoelectric ceramic material and adjusting its electrical properties at the microscopic level. (Li 1-z Ag z )SbO3 as a flux can well improve the sintering characteristics of KNN ceramics, and by doping solid solution Ag elements, the sintering temperature of the ceramics can be reduced, the volatilization of alkali metals can be controlled, the density of piezoelectric ceramics can be increased, and the piezoelectric properties can be improved. The rare earth elements and trivalent metal elements in the perovskite-type composite oxide can both be solid-dissolved with KNN ceramics and can play a doping and modification role on them, thereby improving their piezoelectric properties. The KNN-based lead-free piezoelectric ceramics prepared by the present invention have excellent piezoelectric properties. 33 It reaches 400pC / N, which is much higher than pure KNN ceramics and has better practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a microscopic morphology of the surface of the KNN-based lead-free piezoelectric ceramic prepared in Example 1. DETAILED DESCRIPTION

[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0026] Embodiment 1:

[0027] A KNN-based lead-free piezoelectric ceramic, the chemical structure of which is shown below:

[0028] 0.9(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05(Li 0.9 Ag 0.1 )SbO3-0.05LaCoO3

[0029] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0030] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0031] Li2CO3, Ag2O, and Sb2O3 were weighed according to the chemical measurement and placed in a ball mill. Anhydrous ethanol was used as the medium and the ball mill was used for 10 hours. The ball-milled raw materials were taken out and dried, and placed in a crucible for pre-calcination at a temperature of 850°C for 2 hours to obtain (Li 0.9 Ag 0.1 )SbO3;

[0032] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3、(Li 0.9 Ag 0.1)SbO3 and LaCoO3 are placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder. To the mixed powder, 8 wt % polyvinyl alcohol solution is added as a binder to make granules, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100 MPa. The green body is first heated to 680°C at a rate of 1°C / min for debinding for 4 hours, and then heated to 1100°C at a rate of 10°C / min for sintering for 4 hours.

[0033] Embodiment 2:

[0034] A KNN-based lead-free piezoelectric ceramic, the chemical structure of which is shown below:

[0035] 0.9(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05(Li 0.9 Ag 0.1 )SbO3-0.05LaCoO3

[0036] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0037] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0038] Li2CO3, Ag2O, and Sb2O3 were weighed according to the chemical measurement and placed in a ball mill. Anhydrous ethanol was used as the medium and the ball mill was used for 10 hours. The ball-milled raw materials were taken out and dried, and placed in a crucible for pre-calcination at a temperature of 850°C for 2 hours to obtain (Li 0.9 Ag 0.1 )SbO3;

[0039] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3、(Li 0.9 Ag 0.1)SbO3 and LaCoO3 are placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder. To the mixed powder, 8wt% polyvinyl alcohol solution is added as a binder to make granules, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100 MPa. The green body is first heated to 650℃ at a rate of 1℃ / min to debind for 5 hours, and then heated to 1050℃ at a rate of 10℃ / min and sintered for 5 hours.

[0040] Embodiment 3:

[0041] A KNN-based lead-free piezoelectric ceramic, the chemical structure of which is shown below:

[0042] 0.9(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05(Li 0.9 Ag 0.1 )SbO3-0.05LaCoO3

[0043] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0044] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0045] Li2CO3, Ag2O, and Sb2O3 were weighed according to the chemical measurement and placed in a ball mill. Anhydrous ethanol was used as the medium and the ball mill was used for 10 hours. The ball-milled raw materials were taken out and dried, and placed in a crucible for pre-calcination at a temperature of 850°C for 2 hours to obtain (Li 0.9 Ag 0.1 )SbO3;

[0046] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3、(Li 0.9 Ag 0.1)SbO3 and LaCoO3 are placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder. To the mixed powder, 8wt% polyvinyl alcohol solution is added as a binder to make granules, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100 MPa. The green body is first heated to 750℃ at a rate of 1℃ / min for debinding for 3 hours, and then heated to 1150℃ at a rate of 10℃ / min for sintering for 3 hours.

[0047] Comparative Example 1:

[0048] It is basically the same as Example 1, except that Ta doping is not performed;

[0049] This embodiment provides a KNN-based lead-free piezoelectric ceramic, whose chemical structure is as follows:

[0050] 0.9(K 0.5 Na 0.5 )NbO3-0.05(Li 0.9 Ag 0.1 )SbO3-0.05LaCoO3

[0051] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0052] K2CO3, Na2CO3, and Nb2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium using a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )NbO3;

[0053] Li2CO3, Ag2O, and Sb2O3 were weighed according to the chemical measurement and placed in a ball mill. Anhydrous ethanol was used as the medium and the ball mill was used for 10 hours. The ball-milled raw materials were taken out and dried, and placed in a crucible for pre-calcination at a temperature of 850°C for 2 hours to obtain (Li 0.9 Ag 0.1 )SbO3;

[0054] According to the stoichiometric weight (K 0.5 Na 0.5 )NbO3、(Li 0.9 Ag 0.1)SbO3 and LaCoO3 are placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder. To the mixed powder, 8 wt % polyvinyl alcohol solution is added as a binder to make granules, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100 MPa. The green body is first heated to 680°C at a rate of 1°C / min for debinding for 4 hours, and then heated to 1100°C at a rate of 10°C / min for sintering for 4 hours.

[0055] Comparative Example 2:

[0056] The method is basically the same as Example 1, except that Ag doping is not performed;

[0057] This embodiment provides a KNN-based lead-free piezoelectric ceramic, whose chemical structure is as follows:

[0058] 0.9(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05LiSbO3-0.05LaCoO3

[0059] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0060] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0061] Li2CO3 and Sb2O3 were weighed according to the chemical measurement and placed in a ball milling jar. Anhydrous ethanol was used as the medium and the ball milling was performed for 10 hours using a planetary ball mill. The ball milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a pre-calcination temperature of 850°C and a pre-calcination time of 2 hours to obtain LiSbO3.

[0062] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15)O3, LiSbO3, and LaCoO3 are placed in a ball mill, milled for 10 hours using anhydrous ethanol as a medium using a planetary ball mill, and dried to obtain a mixed powder, to which 8 wt % polyvinyl alcohol solution is added as a binder for granulation, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100 MPa, the green body is first heated to 680°C at a rate of 1°C / min for debinding for 4 hours, and then heated to 1100°C at a rate of 10°C / min for sintering for 4 hours.

[0063] Comparative Example 3:

[0064] The same as Example 1, except that (Li 0.9 Ag 0.1 )SbO3;

[0065] This embodiment provides a KNN-based lead-free piezoelectric ceramic, whose chemical structure is as follows:

[0066] 0.95(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05LaCoO3

[0067] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0068] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0069] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3 and LaCoO3 are placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder, to which 8wt% polyvinyl alcohol solution is added as a binder for granulation, passed through an 80-mesh sieve, and pressed into a green body at a pressure of 100MPa, the green body is first heated to 680℃ at a rate of 1℃ / min for debinding for 4 hours, and then heated to 1100℃ at a rate of 10℃ / min for sintering for 4 hours.

[0070] Comparative Example 4:

[0071] The method is basically the same as Example 1, except that LaCoO3 is not added;

[0072] This embodiment provides a KNN-based lead-free piezoelectric ceramic, whose chemical structure is as follows:

[0073] 0.95(K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3-0.05(Li 0.9 Ag 0.1 )SbO3

[0074] Preparation method of the above-mentioned KNN-based lead-free piezoelectric ceramic:

[0075] K2CO3, Na2CO3, Nb2O5, and Ta2O5 were weighed according to the chemical measurement and placed in a ball mill. They were milled for 10 h using anhydrous ethanol as the medium in a planetary ball mill. The milled raw materials were taken out and dried, and then placed in a crucible for pre-calcination at a temperature of 850°C for 2 h to obtain (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3;

[0076] Li2CO3, Ag2O, and Sb2O3 were weighed according to the chemical measurement and placed in a ball mill. Anhydrous ethanol was used as the medium and the ball mill was used for 10 hours. The ball-milled raw materials were taken out and dried, and placed in a crucible for pre-calcination at a temperature of 850°C for 2 hours to obtain (Li 0.9 Ag 0.1 )SbO3;

[0077] According to the stoichiometric weight (K 0.5 Na 0.5 )(Nb 0.85 Ta 0.15 )O3、(Li 0.9 Ag 0.1 )SbO3 is placed in a ball mill, milled for 10 hours with a planetary ball mill using anhydrous ethanol as a medium, and dried to obtain a mixed powder, to which 8wt% polyvinyl alcohol solution is added as a binder for granulation, passed through an 80-mesh sieve, and pressed into a green body under a pressure of 100MPa, the green body is first heated to 680℃ at a rate of 1℃ / min for debinding for 4 hours, and then heated to 1100℃ at a rate of 10℃ / min for sintering for 4 hours.

[0078] Performance Test:

[0079] The surfaces of the KNN-based lead-free piezoelectric ceramics prepared in Examples 1-3 of the present invention and Comparative Examples 1-4 were polished, coated with silver paste on both sides, kept at 750° C. for 10 min, then polarized at a DC voltage of 4 kV / mm for 20 min in silicone oil at 120° C., and then placed for 24 hours as test pieces to test their electrochemical properties;

[0080] Adopt ZJ-3AN quasi-static d 33 The tester measures the room temperature piezoelectric constant of the specimen;

[0081] The electromechanical coupling coefficient kp, mechanical quality factor Qm and dielectric loss tanδ of the specimen were measured and analyzed using a precision impedance analyzer (Agilent HP4294A) (25°C, 1V, 1kHz)

[0082] Where, the piezoelectric strain constant d 33 The larger the value, the higher the piezoelectric performance. The larger the mechanical quality factor Qm, the smaller the loss of the piezoelectric ceramic during resonant vibration. The electromechanical coupling coefficient kp indicates the energy efficiency ratio of the piezoelectric vibrator in converting mechanical energy into electrical energy or converting electrical energy into mechanical energy during vibration. The dielectric loss tanδ is the energy lost in the dielectric due to polarization relaxation and leakage conduction under the action of the electric field.

[0083] The test results are shown in Table 1 below:

[0084] Table 1:

[0085]

[0086] As shown in Table 1 above, the KNN-based lead-free piezoelectric ceramics prepared in the present invention have excellent piezoelectric properties. 33 It reaches 400pC / N, which is much higher than pure KNN ceramics and has better practical application prospects.

[0087] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A KNN-based lead-free piezoelectric ceramic, characterized in that: Its chemical structure is shown below: (1-a-b)(K) 1-x Na x )(Nb 1-y The y )O3-α(Li 1-z Ag z )SbO3-βNMO3 Among them, 0.3≤x≤0.6, 0<y≤0.3, 0<z≤0.3; 0<α≤0.1,0<β≤0.1; N is a rare earth element; M is a trivalent metal element.

2. The KNN-based lead-free piezoelectric ceramic according to claim 1, characterized in that: 0.45≤x≤0.55, 0.1≤y≤0.2, 0.05≤z≤0.

15.

3. The KNN-based lead-free piezoelectric ceramic according to claim 2, characterized in that: x=0.5, y=0.15, z=0.

1.

4. The KNN-based lead-free piezoelectric ceramic according to claim 1, characterized in that: 0.03≤α≤0.06,0.03≤β≤0.06。 5. The KNN-based lead-free piezoelectric ceramic according to claim 4, characterized in that: α=0.05,β=0.05。 6. The KNN-based lead-free piezoelectric ceramic according to claim 1, characterized in that: N is La.

7. The KNN-based lead-free piezoelectric ceramic according to claim 1, characterized in that: M is Al, Fe or Co.

8. A method for preparing a KNN-based lead-free piezoelectric ceramic according to any one of claims 1 to 7, characterized in that: According to the stoichiometric 1-x Na x )(Nb 1-y Ta y )O3、(Li 1-z Ag z )SbO3 and NMO3 are mixed and ball-milled and then dried to obtain a mixed powder, the mixed powder is granulated, sieved, and pressed into a green body, and the green body is heated to remove binder and then sintered.

9. The method for preparing the KNN-based lead-free piezoelectric ceramic according to claim 8, characterized in that: The debinding temperature is 650-750℃ and the debinding time is 1-5h.

10. The method for preparing the KNN-based lead-free piezoelectric ceramic according to claim 8, characterized in that: The sintering temperature is 1050-1150°C and the sintering time is 1-5h.