Method for preparing Si3N4-Si2N2O-based wave-transparent ceramic material through normal-pressure sintering
Through the normal pressure sintering and the use of gel liquid system, the problem of poor density of Si3N4-Si2N2O ceramics is solved, and its high-temperature mechanical properties and oxidation resistance are improved, and the high-strength and high-density Si3N4-Si2N2O base permeability is achieved. Preparation of wave ceramic materials.
Patent Information
- Application Number
- CN202410919938.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing Si3N4-Si2N2O ceramics have poor sintering density, resulting in poor high-temperature mechanical properties and oxidation resistance. The traditional preparation method is complex and prone to residual SiO2.
By adopting the normal pressure sintering method, Si2N2O powder is sintered evenly and then sintered, and sintering aid and initiator are added to the gel liquid to perform pre-sintering and high-temperature normal pressure sintering to inhibit the decomposition of Si2N2O. Improve the density and mechanical properties of Si3N4-Si2N2O ceramics.
The purity of Si2N2O powder and the mechanical properties of Si3N4-Si2N2O ceramics are improved, and the dependence on equipment is reduced, and a high-strength and high-density Si3N4-Si2N2O base wave-transmissive ceramic material is obtained.
Smart Images

Figure CN118930283A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic material powder preparation and ceramic material preparation, and more specifically to a Si3N4-Si2N2O-based wave-transmitting ceramic material and a preparation method thereof. Background Art
[0002] Si2N2O has low dielectric constant and dielectric loss, excellent high-temperature mechanical properties, oxidation resistance and thermal shock resistance, and shows great potential in the field of high-temperature wave-transmitting materials. Si3N4 has the characteristics of high hardness, high strength, and small thermal expansion coefficient. Especially under high temperature conditions, silicon nitride ceramic materials show excellent high-temperature resistance, chemical inertness to metals, ultra-high hardness and fracture toughness. The Si3N4-Si2N2O-based wave-transmitting ceramic material obtained by combining the two further improves the mechanical properties while maintaining excellent high-temperature wave-transmitting performance.
[0003] Ohashi et al. studied the effect of different sintering aid oxides on the synthesis of Si2N2O by liquid phase reaction. The results showed that Si2N2O is formed by the reaction of SiO2 and Si3N4, and its formation rate is affected by the liquid phase components. Equimolar MgO has a greater promoting effect on the formation of Si2N2O than equimolar ZrO2, 1 / 2Al2O3, 1 / 2Ln2O3 and PSZ. With the increase of the amount of sintering aid added, the high-temperature liquid phase increases during the sintering process, and the intergranular phase also increases after cooling, resulting in the deterioration of the high-temperature mechanical properties and oxidation resistance of Si2N2O ceramics. Huang Zhengyu et al. prepared Si2N2O and α-Si3N4 synergistically toughened Si3N4 ceramics by gel injection molding and pressureless sintering process, adding 5wt.% Si2N2O seeds. The traditional preparation method uses Si3N4 and SiO2 as raw materials to generate Si2N2O. This method of preparing Si3N4-Si2N2O composite ceramics using Si3N4 as raw material has the following problems: additional SiO2 needs to be added, the preparation method is complicated, and SiO2 is easily left in the final product.
[0004] Patent CN102807389A discloses a method for preparing a Si3N4-Si2N2O porous composite ceramic, which comprises mixing Si3N4 and a dispersant and other reactants into a slurry, drying and static pressing to obtain a green body, and performing pressureless sintering on the green body to obtain a Si3N4-Si2N2O porous composite ceramic. However, the mixed slurry formed by the patent has poor dispersion and uniformity, which will lead to insufficient subsequent reactions. In the sintering stage, the temperature stage gradient is not refined, and it is difficult to control the decomposition of Si2N2O and the generation of Si3N4, which reduces the density of Si3N4-Si2N2O and affects its performance. Summary of the invention
[0005] The present invention provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by sintering at normal pressure in order to overcome the problem of poor sintering density of existing Si3N4-Si2N2O ceramics.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering, characterized in that it comprises the following steps:
[0008] S1. The raw materials Si powder and SiO powder are uniformly mixed according to the mass ratio, vacuumed and then introduced into N2, sintered at 1400-1450°C to obtain a coarse powder, and then added with alcohol and a dispersant to grind to obtain Si2N2O powder;
[0009] S2. The Si2N2O powder and the sintering aid are mixed with an organic matter to form a gel liquid;
[0010] S3. adding an initiator to the gel liquid to form a body;
[0011] S4. Pre-sintering treatment of the embryo: heating from 40℃ to 150-160℃, heating rate 0.5-3℃ / min, keeping warm for 10-20min; heating from 200℃ to 350-400℃, heating rate 3-7℃ / min, keeping warm for 20-30min; heating from 420℃ to 750-800℃, heating rate 3-7℃ / min, keeping warm for 10-20min; heating rate 3-7℃ / min, finally keeping warm at 1100-1300℃ for 0.5-1h.
[0012] S5. The pre-sintered green body is subjected to high-temperature normal pressure sintering: in a N2 atmosphere at 0.02-0.05 MPa, the temperature is increased to 550-600°C at a heating rate of 3-7°C / min; the temperature is increased to 950-1000°C at a heating rate of 10°C / min, and the temperature is increased to 1400-1600°C at a heating rate of 3-7°C / min, and the temperature is kept for 1-2 hours.
[0013] Furthermore, the content of the dispersant added in step S1 is 2 wt.%.
[0014] Furthermore, the mass ratio of Si powder, SiO powder and alcohol is 1:1:2.
[0015] Furthermore, the sintering stage in step S1 includes: pumping the gas pressure to -0.25 MPa and then introducing N2 to return it to normal pressure, and raising the sintering temperature to 550-600°C at a heating rate of 3-7°C / min, to 950-1000°C at a heating rate of 10°C / min, and to 1400-1450°C at a heating rate of 5°C / min and keeping it warm for 1-2 hours.
[0016] Furthermore, the content of sintering aid is 5wt.% MgO, 9wt.% Y2O3, and the content of organic matter is 20wt.%.
[0017] Furthermore, the organic matter is a monomer, a cross-linking agent, a dispersant, an initiator, and a catalyst, and the mass ratio thereof is 8:8:2:1:1.
[0018] Furthermore, the sintering aid is one or more of MgO and Y2O3; the monomer is one or more of acrylic acid and dimethylacrylamide; the cross-linking agent is N,N-methyleneacrylamide; the dispersant is one or more of polyethylene glycol, polyethylene glycol, and ammonium polyacrylate; the catalyst is tetramethylethylenediamine; and the initiator is one or more of potassium persulfate and sodium persulfate.
[0019] Furthermore, the average particle size of the Si2N2O powder is less than 10 μm.
[0020] Furthermore, the mass ratio of the gel liquid to the initiator in S3 is 8:1.
[0021] A Si3N4-Si2N2O-based wave-transmitting ceramic material obtained by the above preparation method.
[0022] Compared with the prior art, the beneficial effects are:
[0023] The present invention uses Si2N2O powder generated by the reaction of Si powder and SiO powder under normal pressure, which improves the powder purity of Si2N2O and reduces the dependence on equipment. The present invention uses a gel liquid system to evenly disperse Si2N2O powder and sintering aids. After the embryo is pre-sintered, it is sintered at 1450°C in a N2 atmosphere to reduce the decomposition of Si2N2O. At the same time, the formation of lattice oxygen is inhibited in the N2 environment, so that the pre-sintered Si3N4 is converted into β-phase Si3N4, which better improves the mechanical properties of Si3N4-Si2N2O-based wave-transmitting ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The XRD spectrum of the Si3N4-Si2N2O high temperature resistant wave-transmitting ceramic prepared in Example 1;
[0025] Figure 2 This is the SEM spectrum of the Si3N4-Si2N2O high temperature resistant and wave-transmitting ceramic prepared in Example 1. DETAILED DESCRIPTION
[0026] In order to clearly illustrate the technical features of the present solution, the present invention is described in detail below through specific implementation methods and in conjunction with the accompanying drawings. In the following description, many specific details are described to facilitate a full understanding of the present application. However, the present application can also be implemented in other ways different from those described herein. Therefore, the protection scope of the present application is not limited by the specific embodiments disclosed below.
[0027] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0029] Example 1
[0030] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0031] Preparation of S1 Si2N2O powder: Take Si powder and SiO powder with a molar ratio of 1:1, mix them evenly in a planetary ball mill, place them in a tubular furnace, pump the air pressure in the corundum tube to -0.25MPa and then introduce N2 to return it to normal pressure. The sintering parameters are as follows: heat up to 600℃ at a heating rate of 5℃ / min, heat up to 1000℃ at a heating rate of 10℃ / min, heat up to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, ball-mill the coarse powder and alcohol in a mass ratio of 1:2 and a dispersant content of 2wt.% in a ball mill, and then dry and sieve.
[0032] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0033] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0034] S4 dehydration and degreasing and introduction of Si3N4: slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete degreasing; heat at a rate of 5℃ / min to 1200℃ and keep warm for 1h, introduce Si3N4 and keep the green body at a certain strength, and cool to room temperature with the furnace.
[0035] S5 high temperature sintering: Sinter at normal pressure at 1400℃~1600℃, under N2 atmosphere protection at 0.05MPa, increase the temperature to 600℃ at a heating rate of 5℃ / min, increase the temperature to 1000℃ at a heating rate of 10℃ / min, and increase the temperature to 1450℃ at a heating rate of 5℃ / min and keep it warm for 2h.
[0036] Example 2
[0037] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0038] Preparation of S1 Si2N2O powder: Take Si powder and SiO powder with a molar ratio of 2:1, mix them evenly in a planetary ball mill, place them in a tubular furnace, pump the air pressure in the corundum tube to -0.25MPa and then introduce N2 to return it to normal pressure. The sintering parameters are as follows: heat up to 600℃ at a heating rate of 5℃ / min, heat up to 1000℃ at a heating rate of 10℃ / min, heat up to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, ball-mill the coarse powder and alcohol in a mass ratio of 1:2 and a dispersant content of 2wt.% in a ball mill, and then dry and sieve.
[0039] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0040] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0041] S4 dehydration and degreasing and introduction of Si3N4: slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete degreasing; heat at a rate of 5℃ / min to 1200℃ and keep warm for 1h, introduce Si3N4 and keep the green body at a certain strength, and cool to room temperature with the furnace.
[0042] S5 high temperature sintering: Sinter at normal pressure at 1400℃~1600℃, under N2 atmosphere protection at 0.05MPa, increase the temperature to 600℃ at a heating rate of 5℃ / min, increase the temperature to 1000℃ at a heating rate of 10℃ / min, and increase the temperature to 1450℃ at a heating rate of 5℃ / min and keep it warm for 2h.
[0043] Example 3
[0044] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0045] Preparation of S1 Si2N2O powder: Take Si powder and SiO powder with a molar ratio of 1:2, mix them evenly in a planetary ball mill, place them in a tubular furnace, pump the air pressure in the corundum tube to -0.25MPa and then introduce N2 to return it to normal pressure. The sintering parameters are as follows: heat to 600℃ at a heating rate of 5℃ / min, heat to 1000℃ at a heating rate of 10℃ / min, heat to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, ball-mill the coarse powder and alcohol in a mass ratio of 1:2 and a dispersant content of 2wt.% in a ball mill, and then dry and sieve.
[0046] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0047] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0048] S4 dehydration and degreasing and introduction of Si3N4: slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete degreasing; heat at a rate of 5℃ / min to 1200℃ and keep warm for 1h, introduce Si3N4 and keep the green body at a certain strength, and cool to room temperature with the furnace.
[0049] S5 high temperature sintering: Sinter at normal pressure at 1400℃~1600℃, under N2 atmosphere protection at 0.05MPa, increase the temperature to 600℃ at a heating rate of 5℃ / min, increase the temperature to 1000℃ at a heating rate of 10℃ / min, and increase the temperature to 1450℃ at a heating rate of 5℃ / min and keep it warm for 2h.
[0050] Example 4
[0051] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0052] Preparation of S1 Si2N2O powder: Take Si powder and SiO powder with a molar ratio of 1:1, mix them evenly in a planetary ball mill, place them in a tubular furnace, pump the air pressure in the corundum tube to -0.25MPa and then introduce N2 to return it to normal pressure. The sintering parameters are as follows: heat up to 600℃ at a heating rate of 5℃ / min, heat up to 1000℃ at a heating rate of 10℃ / min, heat up to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, ball-mill the coarse powder and alcohol in a mass ratio of 1:2 and a dispersant content of 2wt.% in a ball mill, and then dry and sieve.
[0053] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0054] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0055] S4 Dehydration and defatting: Slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete defatting.
[0056] S5 high temperature sintering: Sintering was carried out under normal pressure under N2 atmosphere protection at 0.05MPa, with the temperature rising to 600°C at a heating rate of 5°C / min, rising to 1000°C at a heating rate of 10°C / min, and rising to 1450°C at a heating rate of 5°C / min and keeping warm for 2h.
[0057] Example 5
[0058] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0059] Preparation of S1 Si2N2O powder: Take Si3N4 powder and Si powder with a molar ratio of 1:1, place them in a muffle furnace under air atmosphere: heat up to 600℃ at a heating rate of 5℃ / min, heat up to 1000℃ at a heating rate of 10℃ / min, heat up to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, add alcohol and dispersant to ball mill in a ball mill, and then dry and sieve.
[0060] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0061] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0062] S4 dehydration and degreasing and introduction of Si3N4: slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete degreasing; heat at a rate of 5℃ / min to 1200℃ and keep warm for 1h, introduce Si3N4 and keep the green body at a certain strength, and cool to room temperature with the furnace.
[0063] S5 high temperature sintering: sintering at 1400℃~1600℃, 0.05MPa N2 atmosphere protection, heating to 600℃ at a rate of 5℃ / min, heating to 1000℃ at a rate of 10℃ / min, heating to 1450℃ at a rate of 5℃ / min and keeping at this temperature for 2h
[0064] Example 6
[0065] This embodiment provides a method for preparing Si3N4-Si2N2O-based wave-transmitting ceramics, comprising the following steps:
[0066] Preparation of S1 Si2N2O powder: Take Si powder and SiO powder with a molar ratio of 1:1, mix them evenly in a planetary ball mill, place them in a tubular furnace, pump the air pressure in the corundum tube to -0.25MPa and then introduce N2 to return it to normal pressure. The sintering parameters are as follows: heat up to 600℃ at a heating rate of 5℃ / min, heat up to 1000℃ at a heating rate of 10℃ / min, heat up to 1450℃ at a heating rate of 5℃ / min and keep warm for 2h, cool to room temperature with the furnace to obtain coarse powder, ball-mill the coarse powder and alcohol in a mass ratio of 1:2 and a dispersant content of 2wt.% in a ball mill, and then dry and sieve.
[0067] S2 gel liquid for Si2N2O powder dispersion, homogenization and molding: add 5wt.% MgO, 9wt.% Y2O3; monomers are acrylic acid (AA), dimethyl acrylamide (DMAA); crosslinker N,N-methylene acrylamide (MBAM); initiator ammonium sulfate (APS), redox initiator (sodium pyrosulfite) one or more; dispersant polyethylene glycol (PEG400), polyethylene glycol (PEG1000), ammonium polyacrylate (NH4PAA). The total amount of organic matter accounts for 20wt.% of the powder mass; finally, add Si2N2O powder and sintering aid to the organic mixture, mix evenly in a heating and stirring device to form a gel state.
[0068] S3 molding: add initiator (ratio of 1:1, total amount of 1wt.%) potassium persulfate, sodium persulfate, catalyst (1wt.%) tetramethylethylenediamine, and heat to 50°C to mix; finally, inject and solidify into a block.
[0069] S4 dehydration and degreasing and introduction of Si3N4: slowly dehydrate and remove part of the lipids at 40-160℃ for 10h; heating rate 5℃ / min, and keep warm twice at 200-400℃ and 420-800℃ respectively to ensure complete degreasing; heat at a rate of 5℃ / min to 1300℃ and keep warm for 2h, introduce Si3N4 and keep the green body at a certain strength, and cool to room temperature with the furnace.
[0070] S5 high temperature sintering: Sinter at normal pressure at 1400℃~1600℃, under N2 atmosphere protection at 0.05MPa, increase the temperature to 600℃ at a heating rate of 5℃ / min, increase the temperature to 1000℃ at a heating rate of 10℃ / min, and increase the temperature to 1450℃ at a heating rate of 5℃ / min and keep it warm for 2h.
[0071] The performance of the Si3N4-Si2N2O-based wave-transmitting ceramics prepared in Implementations 1 to 6 was tested, and the various properties are shown in Table 1.
[0072] Table 1
[0073] Flexural strength(MPa) Dielectric constant <![CDATA[Loss tangent (10 -3 )]]> Example 1 408 4.0 3.2 Example 2 417 4.3 3.4 Example 3 368 4.5 3.7 Example 4 386 5.0 3.9 Example 5 421 4.6 3.7 Example 6 435 4.7 3.8
[0074] From Table 1 and Figure 1 It can be seen that in Example 1, Si2N2O powder is prepared by sintering Si powder and SiO powder, and then the powder is dispersed and homogenized to form a gel liquid. Then, an initiator is added to the gel liquid, and a physical and chemical reaction occurs in the corresponding mold cavity to form a high-strength green body in situ. The green body is then pre-sintered to decompose a small part of Si2N2O to obtain Si3N4. Finally, it is sintered at high temperature and normal pressure under a nitrogen atmosphere to inhibit the decomposition of Si2N2O and densify it, thereby obtaining Si3N4-Si2N2O high temperature resistant and wave-transmitting ceramics with good mechanical properties and high flexural strength.
[0075] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-limiting from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and any reference numerals in the claims should not be regarded as limiting the claims involved.
Claims
1. A method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic materials by atmospheric pressure sintering, characterized in that: The steps include: S1. The raw materials Si powder and SiO powder are uniformly mixed according to the mass ratio, vacuumed and then introduced into N2, sintered at 1400-1450°C to obtain a coarse powder, and then added with alcohol and a dispersant to grind to obtain Si2N2O powder; S2. The Si2N2O powder and the sintering aid are mixed with an organic matter to form a gel liquid; S3. adding an initiator to the gel liquid to form a body; S4. Pre-sintering treatment of the embryo: heating from 40°C to 150-160°C, heating rate 0.5-3°C / min, keeping warm for 10-20min; heating from 200°C to 350-400°C, heating rate 3-7°C / min, keeping warm for 20-30min; heating from 420°C to 750-800°C, heating rate 3-7°C / min, keeping warm for 10-20min; The heating rate is 3-7°C / min, and finally the temperature is kept at 1100-1300°C for 0.5-1h. S5. The pre-sintered green body is subjected to high-temperature normal pressure sintering: in a N2 atmosphere at 0.02-0.05 MPa, the temperature is increased to 550-600°C at a heating rate of 3-7°C / min; the temperature is increased to 950-1000°C at a heating rate of 10°C / min, and the temperature is increased to 1400-1600°C at a heating rate of 3-7°C / min, and the temperature is kept for 1-2 hours.
2. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The content of the dispersant added in step S1 is 2 wt.%.
3. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: In the step S1, the mass ratio of Si powder, SiO powder and alcohol is 1:1:
2.
4. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The sintering stage in step S1 includes: pumping the gas pressure to -0.25MPa and then introducing N2 to return it to normal pressure, raising the sintering temperature to 550-600°C at a heating rate of 3-7°C / min, to 950-1000°C at a heating rate of 10°C / min, to 1400-1450°C at a heating rate of 5°C / min and keeping it warm for 1-2h.
5. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The sintering aid content is 5wt.% MgO, 9wt.% Y2O3, and the organic matter content is 20wt.%.
6. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by sintering Si and SiO powder under normal pressure according to claim 4, characterized in that: The organic substances include monomers, cross-linking agents, dispersants, initiators and catalysts, and the mass ratio thereof is 8:8:2:1:
1.
7. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The sintering aid is one or more of MgO and Y2O3; the monomer is one or more of acrylic acid and dimethyl acrylamide; the cross-linking agent is N,N-methylene acrylamide; the dispersant is one or more of polyethylene glycol, polyethylene glycol, and ammonium polyacrylate; the catalyst is tetramethylethylenediamine; and the initiator is one or more of potassium persulfate and sodium persulfate.
8. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The average particle size of the Si2N2O powder is less than 10 μm.
9. The method for preparing Si3N4-Si2N2O-based wave-transmitting ceramic material by atmospheric pressure sintering according to claim 1, characterized in that: The mass ratio of the gel liquid to the initiator in the S3 is 8:
1.
10. The Si3N4-Si2N2O-based wave-transmitting ceramic material obtained according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of near net-shape of porous silicon nitride / silicon oxynitride ceramic composite material
CN101531538A
Porous Si2N2O high temperature-resistant wave-permeable ceramics and preparation method thereof
CN108752008A
Si2N2O high-temperature-resistant wave-transparent ceramic and preparation method thereof
CN113233904A
Production of fiber-reinforced silicon oxynitride sintered compact
JP1989282154A
Nanoscale ceramic composites and methods of making
US20070142203A1