Method for improving sintering flatness of electrostatic chuck ceramic plate
Through the calculation of the area and design of the partition filler fixture for uniform filling, combined with the hot press sintering of the graphite pad plate, the problem of insufficient thickness uniformity of the ceramic plate is solved, and the high-precision sintering effect of the ceramic plate is achieved, and the thickness uniformity reaches <0.2 mm.
Patent Information
- Application Number
- CN202410864149.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-11-12
AI Technical Summary
In the field of semiconductor-grade precision ceramics with strict ceramic flatness requirements, it is difficult for the prior art to ensure the thickness uniformity of the ceramic electrode layer to the ceramic body. Especially for powders with poor fluidity, the thickness uniformity after sintering is often more than 0.3mm. The requirement of <0.2mm cannot be met.
By calculating the ceramic quality and powder firing loss by region, designing a partition filler fixture for uniform filling, combining a graphite pad for hot pressing and sintering, and detecting the thickness difference on the marble platform to ensure the uniformity of the thickness of the ceramic plate.
The sintering flatness of the ceramic plate is significantly improved, and the thickness uniformity reaches <0.2mm, meeting the use requirements of semiconductor-grade precision ceramic parts.
Smart Images

Figure CN118930284A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sintering electrostatic chuck ceramic plates, in particular to a method for improving the sintering flatness of electrostatic chuck ceramic plates. Background Art
[0002] Semiconductor-grade precision ceramics have strict requirements for ceramic flatness. In the field of ceramic heaters, the thickness uniformity requirement from the ceramic electrode layer to the ceramic body is less than 0.2mm. It is difficult to ensure such flatness requirements during the pressing process. Especially for some powders with poor fluidity, the uneven filling during the filling process is caused by the uneven flow of the powder. This unevenness still exists during the sintering process, resulting in serious thickness uniformity of the ceramic plate after sintering. At present, the better one can achieve less than 0.3mm. Therefore, a method is needed to improve the sintering flatness of the electrostatic chuck ceramic plate. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for improving the sintering flatness of an electrostatic chuck ceramic plate, which can improve the sintering flatness of an electrostatic chuck ceramic plate.
[0004] In order to solve the above technical problems, the technical solution of the present invention is:
[0005] A method for improving the sintering flatness of an electrostatic chuck ceramic plate, the method comprising:
[0006] According to the density and area of the sintered body of the electrostatic chuck ceramic block, the electrostatic chuck ceramic block is first divided into regions, and the ceramic mass of each region is calculated;
[0007] The same degreasing and sintering process as the ceramic block is used to degreasing and sinter the ceramic powder to obtain the loss on ignition ratio of the powder;
[0008] Calculate the mass of the filler in each area. The mass of the powder filling in each area is the ratio of the ceramic mass in each area to the ignition loss of the powder;
[0009] According to the filling powder mass, loose packing density of the powder, and the area size, calculate the filling height H of the area. The filling height H is calculated by the following formula:
[0010] H=(M / ρ) / S
[0011] Among them, H is the packing height, M is the powder filling mass in the area, ρ is the loose packing density of the powder, and S is the area of the area;
[0012] According to the calculation results of the above steps, a partition filler jig is designed, wherein the partition filler jig comprises an outer ring and a plurality of partition ribs arranged in the outer ring, wherein two adjacent partition ribs and a portion of the outer ring sandwiched between the two adjacent partition ribs form a partition, and the partition filler jig is divided into a plurality of regions;
[0013] During the molding process, the partition filling jig is used to add corresponding masses of powders in the respective corresponding areas, and the powders are stirred evenly by a stirring tool. After all areas on the partition filling jig are filled, the partition filling jig is taken out vertically upward, and a tool is used to vertically insert and pull out the partition edge at the original position of the partition edge, so that the powder flows in the gap formed after the partition edge is pulled out, and the gap formed after the partition edge is pulled out is filled;
[0014] Adding a graphite pad, hot pressing and sintering the electrostatic chuck ceramic plate;
[0015] The thickness of the sintered ceramic blocks is tested on a marble platform, and the range of the minimum and maximum thicknesses is calculated.
[0016] Preferably, the outer ring and the partition ribs are both processed through a transparent acrylic plate, and the thickness of the outer ring and the partition ribs are both 0.8-1.2 mm.
[0017] Preferably, the stirring tool is a plastic rod with a diameter of 2 mm.
[0018] Preferably, the tool is a plastic sheet with a length of 30 to 50 mm, a width of 2 to 5 mm, and a thickness of 1 mm.
[0019] Preferably, for an 8-inch electrostatic chuck ceramic plate, the partitioned filler fixture includes a 12-sided outer ring and 6 ribs of equal length, and the angles between any two adjacent ribs are equal.
[0020] Preferably, for a 12-inch electrostatic chuck ceramic plate, the partitioned filling fixture includes a circular outer ring, transverse partition ribs and longitudinal partition ribs, the transverse partition ribs include first transverse partition ribs, second transverse partition ribs and third transverse partition ribs, both ends of the first transverse partition ribs, the second transverse partition ribs and the third transverse partition ribs are connected to the inner side wall of the circular outer ring, the second transverse partition ribs are arranged between the first transverse partition ribs and the third transverse partition ribs, and the first transverse partition ribs and the third transverse partition ribs are symmetrically arranged about the second transverse partition ribs, the longitudinal partition ribs include first longitudinal partition ribs, second longitudinal partition ribs and third longitudinal partition ribs, both ends of the first longitudinal partition ribs, the second longitudinal partition ribs and the third longitudinal partition ribs are connected to the inner side wall of the circular outer ring, the second longitudinal partition ribs are arranged between the first longitudinal partition ribs and the third longitudinal partition ribs, and the first longitudinal partition ribs and the third longitudinal partition ribs are symmetrically arranged about the second longitudinal partition ribs.
[0021] The above technical solution has the following beneficial effects:
[0022] By using a partitioned filling fixture to ensure the filling weight within a certain area, the filling uniformity of the entire ceramic plate can be ensured by ensuring the weight of the ceramic powder in the area, thereby improving the thickness uniformity of the ceramic block after sintering;
[0023] By using the method for improving the sintering flatness of the electrostatic chuck ceramic plate of the present application, the thickness uniformity of the ceramic plate is significantly improved, meeting the use requirements of semiconductor-grade precision ceramic parts, and the thickness uniformity is less than 0.2 mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the structure of the 8-inch electrostatic chuck ceramic plate partition filler fixture of the present invention;
[0025] Figure 2 It is a structural schematic diagram of the 12-inch electrostatic chuck ceramic plate partition filler fixture of the present invention. DETAILED DESCRIPTION
[0026] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0027] A method for improving the sintering flatness of an electrostatic chuck ceramic plate comprises the following steps:
[0028] According to the density and area of the electrostatic chuck ceramic block sintered body, the electrostatic chuck ceramic block is first divided into regions, and the ceramic mass of each region is calculated, so that the ceramic sintered powder can be filled into each region after the division;
[0029] The same degreasing and sintering process as the ceramic block is used to degreasing and sinter the ceramic powder to obtain the loss on ignition ratio of the powder;
[0030] Calculate the mass of the filler in each area. The mass of the powder filling in each area is the ratio of the ceramic mass in each area to the ignition loss of the powder;
[0031] According to the filling powder mass, loose packing density of the powder, and the area size, calculate the filling height H of the area. The filling height H is calculated by the following formula:
[0032] H=(M / ρ) / S
[0033] Among them, H is the packing height, M is the powder filling mass in the area, ρ is the loose packing density of the powder, and S is the area of the area;
[0034] According to the calculation results of the above steps, a partition filler jig is designed, wherein the partition filler jig includes an outer ring and a plurality of partition ribs arranged in the outer ring, wherein two adjacent partition ribs and a portion of the outer ring sandwiched between the two adjacent partition ribs form a partition, and the partition filler jig is divided into a plurality of regions;
[0035] During the molding process, a partition filling jig is used to add corresponding masses of powder to the respective corresponding areas, and the powder is stirred evenly by a stirring tool. After all areas on the partition filling jig are filled, the partition filling jig is taken out vertically upward, and a tool is used to vertically insert and pull out the original partition edge position, so that the powder flows in the gap formed after the partition edge is pulled out, and the gap formed after the partition edge is pulled out is filled;
[0036] Adding a graphite pad, hot pressing and sintering the electrostatic chuck ceramic plate;
[0037] The sintered ceramic blocks are tested for thickness on a marble platform to calculate the range of the minimum and maximum thicknesses.
[0038] The ceramic plate is sintered by the above method, and the thickness uniformity of the sintered ceramic plate is significantly improved, meeting the use requirements of semiconductor-grade precision ceramic parts, and the thickness uniformity is less than 0.2 mm, meeting the flatness requirements of the electrostatic chuck ceramic plate;
[0039] The outer ring and the spacer ribs are processed by transparent acrylic plates, and the thickness of the outer ring and the spacer ribs is 0.8 mm. In other implementations of this embodiment, the thickness of the outer ring and the spacer ribs is 1.2 mm. In other implementations of this embodiment, the outer ring and the spacer ribs can also be made of the same material as the ceramic sintered powder, and are first formed, and then the sintered powder is added, and then they are sintered in the sintering furnace together with the powder;
[0040] Among them, the stirring tool is a plastic rod with a diameter of 2 mm;
[0041] The tool is a plastic sheet with a length of 30 mm, a width of 2 mm, and a thickness of 1 mm. In other implementations of this embodiment, the tool is a plastic sheet with a length of 50 mm, a width of 5 mm, and a thickness of 1 mm.
[0042] refer to Figure 1 In order to process the 8-inch electrostatic chuck ceramic plate, the partition filler fixture includes a 12-sided outer ring 1 and 6 ribs 2 of equal length. In order to facilitate calculation and adding powder, the 12-sided outer ring 1 is a regular 12-sided deformed outer ring. The 6 ribs 2 of equal length converge at the center of the 12-sided outer ring 1. The angles between any two adjacent ribs 2 are equal. After sintering, it is processed into a disc-shaped 8-inch electrostatic chuck ceramic plate. The 6 ribs 2 of equal length divide the interior of the 12-sided outer ring 1 into 6 equal parts. The powder added during sintering is equal.
[0043] In other implementations of this embodiment, 12 spacer ribs 2 may be provided to evenly divide the 12-sided outer ring 1 into 12 equal parts;
[0044] refer to Figure 2 For a 12-inch electrostatic chuck ceramic plate, a partition packing fixture includes a circular outer ring 3, transverse ribs and longitudinal ribs, the transverse ribs include a first transverse rib 4, a second transverse rib 5, and a third transverse rib 6, both ends of the first transverse rib 4, the second transverse rib 5, and the third transverse rib 6 are connected to the inner side wall of the circular outer ring 3, the second transverse rib 5 is arranged between the first transverse rib 4 and the third transverse rib 6, the first transverse rib 4 and the third transverse rib 6 are symmetrically arranged about the second transverse rib 5, the longitudinal ribs include a first longitudinal rib 7, a second longitudinal rib 8, and a third longitudinal rib 9, both ends of the first longitudinal rib 7, the second longitudinal rib 8, and the third longitudinal rib 9 are connected to the inner side wall of the circular outer ring 3, the second longitudinal rib 8 is arranged between the first longitudinal rib 7 and the third longitudinal rib 9, and the first longitudinal rib 7 and the third longitudinal rib 9 are symmetrically arranged about the second longitudinal rib 8;
[0045] The first transverse partition rib 4, the second transverse partition rib 5, and the third transverse partition rib 6 intersect with the first longitudinal partition rib 7, the second longitudinal partition rib 8, and the third longitudinal partition rib 9 respectively, and the distance between the first transverse partition rib 4 and the second transverse partition rib 5 is equal to the distance between the second transverse partition rib 5 and the third transverse partition rib 6. Correspondingly, the first longitudinal partition rib 7, the second longitudinal partition rib 8, and the third longitudinal partition rib 9 intersect with the first transverse partition rib 4, the second transverse partition rib 5, and the third transverse partition rib 6 respectively, and the distance between the first longitudinal partition rib 7 and the second longitudinal partition rib 8 is equal to the distance between the second longitudinal partition rib 8 and the third longitudinal partition rib 9. By segmenting by the above method, four square blocks 10 with the same area, four large side blocks 11 with the same area, and four small side blocks 12 with the same area are obtained, and it is relatively easy to calculate the amount of powder in each area;
[0046] By using a partitioned filling fixture to ensure the filling weight within a certain area, the filling uniformity of the entire ceramic plate can be ensured by ensuring the weight of the ceramic powder in the area, thereby improving the thickness uniformity of the ceramic block after sintering;
[0047] By using the method for improving the sintering flatness of the electrostatic chuck ceramic plate of the present application, the thickness uniformity of the ceramic plate is significantly improved, meeting the use requirements of semiconductor-grade precision ceramic parts, and the thickness uniformity is less than 0.2 mm.
[0048] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
Claims
1. A method for improving the sintering flatness of an electrostatic chuck ceramic plate, characterized in that: The method comprises: According to the density and area of the sintered body of the electrostatic chuck ceramic block, the electrostatic chuck ceramic block is first divided into regions, and the ceramic mass of each region is calculated; The same degreasing and sintering process as the ceramic block is used to degreasing and sinter the ceramic powder to obtain the loss on ignition ratio of the powder; Calculate the mass of the filler in each area. The mass of the powder filling in each area is the ratio of the ceramic mass in each area to the ignition loss of the powder; According to the filling powder mass, loose packing density of the powder, and the area size, calculate the filling height H of the area. The filling height H is calculated by the following formula: H=(M / ρ) / S Among them, H is the packing height, M is the powder filling mass in the area, ρ is the loose packing density of the powder, and S is the area of the area; According to the calculation results of the above steps, a partition filler jig is designed, wherein the partition filler jig comprises an outer ring and a plurality of partition ribs arranged in the outer ring, wherein two adjacent partition ribs and a portion of the outer ring sandwiched between the two adjacent partition ribs form a partition, and the partition filler jig is divided into a plurality of regions; During the molding process, the partition filling jig is used to add corresponding masses of powders in the respective corresponding areas, and the powders are stirred evenly by a stirring tool. After all areas on the partition filling jig are filled, the partition filling jig is taken out vertically upward, and a tool is used to vertically insert and pull out the partition edge at the original position of the partition edge, so that the powder flows in the gap formed after the partition edge is pulled out, and the gap formed after the partition edge is pulled out is filled; Adding a graphite pad, hot pressing and sintering the electrostatic chuck ceramic plate; The thickness of the sintered ceramic blocks is tested on a marble platform, and the range of the minimum and maximum thicknesses is calculated.
2. A method for improving the sintering flatness of an electrostatic chuck ceramic plate according to claim 1, characterized in that: The outer ring and the partition ribs are both processed through a transparent acrylic plate, and the thickness of the outer ring and the partition ribs are both 0.8-1.2 mm.
3. A method for improving the sintering flatness of an electrostatic chuck ceramic plate according to claim 1, characterized in that: The stirring tool is a plastic rod with a diameter of 2 mm.
4. A method for improving the sintering flatness of an electrostatic chuck ceramic plate according to claim 1, characterized in that: The tool is a plastic sheet with a length of 30 to 50 mm, a width of 2 to 5 mm and a thickness of 1 mm.
5. A method for improving the sintering flatness of an electrostatic chuck ceramic plate according to claim 1, characterized in that: For an 8-inch electrostatic chuck ceramic plate, the partition filler fixture includes a 12-sided outer ring and 6 ridges of equal length, and the angles between any two adjacent ridges are equal.
6. A method for improving the sintering flatness of an electrostatic chuck ceramic plate according to claim 1, characterized in that: For a 12-inch electrostatic chuck ceramic plate, the partitioned filling fixture includes a circular outer ring, transverse ribs and longitudinal ribs, the transverse ribs include first transverse ribs, second transverse ribs and third transverse ribs, both ends of the first transverse ribs, the second transverse ribs and the third transverse ribs are connected to the inner side wall of the circular outer ring, the second transverse ribs are arranged between the first transverse ribs and the third transverse ribs, the first transverse ribs and the third transverse ribs are symmetrically arranged about the second transverse ribs, the longitudinal ribs include first longitudinal ribs, second longitudinal ribs and the third longitudinal ribs, both ends of the first longitudinal ribs, the second longitudinal ribs and the third longitudinal ribs are connected to the inner side wall of the circular outer ring, the second longitudinal ribs are arranged between the first longitudinal ribs and the third longitudinal ribs, and the first longitudinal ribs and the third longitudinal ribs are symmetrically arranged about the second longitudinal ribs.
Citation Information
Patent Citations
Device and method for forming pattern in specific thickness ceramic tile or slab
CN101186080A
Electrostatic chuck
CN103180266A
Rapid pressing method for large-length-diameter-ratio heat-proof layer and metal piece integrally-formed heat-proof product for aerospace vehicle and product thereof
CN114571649A
Silicon nitride sintered substrate, silicon nitride sintered substrate sheet, circuit substrate, and production method for silicon nitride sintered substrate