High-temperature refractory mortar with controllable expansibility and preparation method thereof

Through vacuum impregnation treatment and process optimization, high-temperature refractory mud with controllable expansion is prepared, which solves the shrinkage and gap problems of refractory mud at high temperature, and improves safety and environmental protection. It is suitable for the tantrum between the in-bet water outlet and the seat brick. Fire mud cracks.

CN118930291APending Publication Date: 2024-11-12JIANGSU JIANAI HIGH TEMPERATURE MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411112434.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing high-temperature refractory mud is prone to over-shrinkage or gaps under high temperature conditions, which affects its safety of use, and the existing methods of controlling expansion are costly and difficult to achieve industrialization.

Method used

The hot brick recycled material after vacuum impregnation, mule sand raw material, aluminum waste and other raw materials are prepared through vacuum impregnation and stirring processes, and high-temperature refractory mud with controllable expansion is prepared. Form the 'core-shell' structure of mullite-muled sand, controlling the expansion coefficient and construction properties.

Benefits of technology

It realizes controllable expansion at high temperatures, tight filling gaps, improves usage safety, reduces primary resource consumption, and avoids industrial solid waste pollution. It is suitable for the fire mud joint between the in-between water outlet and the seat brick.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of refractory materials, and particularly discloses expansibility-controllable high-temperature refractory mortar which comprises the following components: 30-70 wt% of runner brick reclaimed materials subjected to vacuum impregnation treatment, 10-60 wt% of mullite sand raw materials, 1-6 wt% of Guangxi mud and 3-9 wt% of aluminum waste, and the total amount of the raw materials is 100 wt%. According to the invention, the recovered runner brick subjected to vacuum impregnation treatment, the aluminum waste material and the mullite sand are used as the raw materials, so that the environmental pollution caused by stacking of a large amount of solid waste is solved; and moreover, due to the volume expansion effect accompanied by phase change of the mullite sand under the high-temperature condition, fireclay gaps can be filled more tightly, and the problem of steel seepage caused by fireclay shrinkage or untight filling under the high-temperature condition is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, and specifically relates to a high-temperature refractory clay with controllable expansion performance and a preparation method thereof. Background Art

[0002] Refractory clay, also known as fire clay or joint material, is a high-temperature resistant material used in the production or construction process of refractory materials to fill gaps. According to the material, high-temperature refractory clay can be divided into clay, magnesium, high-aluminum, corundum, chrome corundum, etc. High-temperature refractory clay must have the following characteristics during use: ① Good plasticity and adhesion, which is convenient for construction and ensures the tightness of fire clay gaps; ② Good high-temperature resistance and controllable expansion. Excellent high-temperature physical properties are the prerequisites for the use of refractory clay in high-temperature environments. Controllable expansion under high-temperature conditions can fill the gaps caused by the sintering and shrinkage of other components in the refractory clay at high temperatures, which can improve the safety factor of the refractory clay during use; ③ Excellent corrosion resistance.

[0003] At present, China's economy is in a period of growth, which brings with it high energy consumption, high pollution, and restrictions on resources and environmental conditions. A large number of workers are calling for a change in the current economic model. An important part of the development of circular economy in the refractory industry is the recycling of solid waste; reducing the consumption of primary resources has important practical significance for improving the current shortage of mineral resources in China. Therefore, the recycling and reuse of refractory materials and the utilization of industrial solid waste are the only way for the sustainable development of refractory materials.

[0004] When high-temperature refractory clay shrinks excessively or has gaps under high temperature conditions, it will affect the safety of its use. For example, during the use of the continuous casting tundish, if the refractory clay between the nozzle and the seat brick is over-sintered or the refractory clay is not filled tightly during construction, it is very easy to cause steel penetration accidents at the refractory clay gap between the seat brick and the nozzle. In the prior art, the micro-expansion of refractory clay is mainly controlled by introducing additives. For example, Chinese patent CN 110423128 A proposes a "method for preparing shrinkage-resistant high-refractory refractory clay". Although it improves the volume stability of refractory clay in high temperature environments, it is difficult to achieve industrialization due to the expensive raw materials such as potassium zirconium phosphate used.

[0005] In view of the above problems, the present invention patent designs a high-temperature refractory clay with controllable expansion and a preparation method thereof, which is specifically applied to the refractory clay joint between the tundish water inlet and the seat brick. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a high-temperature refractory clay with controllable expansion and a preparation method thereof in view of the shortcomings of the above prior art.

[0007] The technical solution of the present invention to solve the above technical problems is: a high-temperature refractory clay with controllable expansion, comprising the following components: 30-70wt·% of recycled Tangdao bricks after vacuum impregnation treatment, 10-60wt·% of mullite raw material, 1-6wt·% of Guangxi mud, 3-9wt·% of aluminum waste, the total amount of the above raw materials is 100wt·%, and 0.1-1wt·% of the total amount of the above raw materials, 0.1-0.8wt·% of the thickener and 2-6wt·% of the binder are added.

[0008] The present invention further defines the scheme: Preferably, the vacuum impregnation treated soup duct brick recycled material is obtained by subjecting the used soup duct bricks to a series of treatment processes such as crushing, screening, magnetic separation, vacuum impregnation, and drying.

[0009] Preferably, the Al2O3 of the recycled soup brick material treated by vacuum impregnation is greater than 70wt·%, the mullite phase content is greater than 90wt·%, the particle size is 1-0.5mm and 0.5-0.2mm, and the specific gravity is 1:2.

[0010] Preferably, the Al2O3 content in the mullite sand raw material is 30-48wt·%, the SiO2 content is 40-60wt·%, the mullite content is greater than 65wt·%, the cristobalite content is 10-20wt·%, and the particle size is 200-325 mesh.

[0011] Preferably, the impregnation liquid required for the vacuum impregnation treatment of the recycled materials of the soup road brick is a mullite material with a solid content of 30-85wt·%, and the vacuum degree required by the vacuum equipment is 10 -3 -10 -5 Pa, vacuum impregnation time is 5-30 minutes.

[0012] Preferably, the aluminum waste is solid waste generated during the smelting process of metallic aluminum, and its Al2O3 content is greater than 65wt·%, the metallic aluminum content is less than 4wt·%, and the particle size is D50 less than 0.088μm.

[0013] Preferably, the Guangxi mud has an Al2O3 content of >20wt·%, a plasticity index of >30, and a particle size of 200-300 mesh.

[0014] Preferably, the dispersant is one or both of water-soluble sodium ammonium acrylate or triethylhexyl phosphate; the thickener is one or both of gelatin or sodium carboxymethyl cellulose; and the binder is one or both of potassium water glass or aluminum dihydrogen phosphate.

[0015] The present invention provides a method for preparing a high-temperature refractory clay with controllable expansion, characterized in that the method comprises the following steps: The first step is to crush, screen and magnetically separate the selected used soup duct bricks to obtain recycled soup duct bricks of different particle sizes; The second step is to use vacuum impregnation method to treat the recycled materials of Tangdao bricks. The impregnation liquid is mullite sand with a solid content of 30-85wt·% and the vacuum degree required by the vacuum equipment is 10 -3 -10 -5 Pa, the vacuum impregnation time is 5-30 minutes, and finally after drying at 110-180°C, the vacuum impregnation pretreated Tangdao brick recycled material is obtained; Step 3: weigh the raw materials according to the fixed ratio; Step 4: Place the fine powder of various raw materials, dispersant and thickener in a ball mill and mix for 2-6 hours to obtain a premixed powder; Step 5: Place the premixed powder and the vacuum impregnation pretreated recycled brick material in a high-powered mixer and stir for 5-20 minutes, then add the binder to obtain the high-temperature refractory mud material.

[0016] The high-temperature refractory clay prepared as described above is applied to the refractory gaps of the inlaid sizing nozzles and the refractory gaps between the nozzle seat brick and the nozzle, and its linear change rate within 1200-1600°C is 0.5%-5%, and when the temperature is higher than 1400°C, the mullite content is greater than 80%. Beneficial Effects

[0017] The present invention uses a vacuum impregnation method to treat the recycled materials of soup bricks and the solid waste generated in the process of metal aluminum smelting as the main raw materials to prepare a high-temperature refractory clay with controllable expansion, which reduces the consumption of primary resources, not only avoids the pollution of the environment by industrial solid waste, but also enhances the use performance of the material, turning waste into treasure, which is of great significance to the sustainable development of the economy.

[0018] The present invention forms a "core-shell" structure of mullite-mullite sand through vacuum impregnation treatment of recycled soup road bricks. Inside the high-temperature refractory fireclay, cristobalite in the mullite sand in the "core-shell" structure reacts with alumina in solid waste generated in the process of metal aluminum smelting. The secondary mullitization causes the fireclay to produce a certain expansion effect, so that the gaps in the fireclay are filled more tightly, thereby improving the safety of the use process and effectively solving the problem of steel infiltration caused by shrinkage or loose filling of the fireclay under high temperature conditions.

[0019] The solid waste generated during the smelting process of the metal aluminum used in the present invention contains a small amount of metal aluminum, which reacts with water in the binder to produce hydrogen, thereby enhancing the air permeability of the fire clay and avoiding cracks during the use of the fire clay.

[0020] The invention optimizes the recycled material processing process and controls the addition amount or addition method of the mullite sand raw material, so that the expansion coefficient of the high-temperature refractory mud at high temperature is controllable, and the high-temperature refractory mud with a suitable expansion coefficient can be selected according to the specific conditions of the construction site.

[0021] The invention uses Guangxi mud, thickener (gelatin or sodium carboxymethyl cellulose) and the like to ensure its workability, uses potassium water glass or aluminum dihydrogen phosphate as a binder to replace tap water, and ensures the medium and high temperature mechanical properties of the high-temperature refractory mud when in use. DETAILED DESCRIPTION Example

[0022] The present embodiment provides a high-temperature refractory mud with controllable expansion, comprising the following components: 50wt·% of recycled Tangdao brick after vacuum impregnation treatment, 40wt·% of mullite raw material, 3wt·% of Guangxi mud, 7wt·% of aluminum waste, the total amount of the above raw materials is 100wt·%, and 0.3wt·% of the total amount of the above raw materials, 0.4wt·% of the thickener and 3wt·% of the binder are added; The Al2O3 of the recycled bricks treated by vacuum impregnation is greater than 70wt·%, and the mullite phase content is greater than 90wt·%; and the recycled bricks are a mixture of 1-0.5mm and 0-0.5mm with a specific gravity of 1:2. The content of Al2O3 in mullite sand is 40wt·%, the content of SiO2 is 60wt·%, the content of mullite is more than 65wt·%, the content of cristobalite is 10wt·%, and the particle size is 250 mesh; Aluminum scrap is solid waste generated during the smelting process of aluminum metal, with Al2O3 content > 65wt·%, aluminum metal content < 4wt·%, and particle size D50 < 0.088μm; Guangxi mud has an Al2O3 content of >20wt·%, a plasticity index of >30, and a particle size of 200 mesh; The dispersant is water-soluble sodium ammonium acrylate; the thickener is sodium carboxymethyl cellulose; and the binder is aluminum dihydrogen phosphate.

[0023] The present embodiment also provides a method for preparing a high-temperature refractory clay with controllable expansion, which specifically comprises the following steps: The first step is to crush, screen and magnetically separate the selected used soup duct bricks to obtain recycled soup duct bricks of different particle sizes; The second step is to use vacuum impregnation method to treat the recycled materials of Tangdao bricks. The impregnation liquid is made of mullite with a solid content of 60wt·% and the vacuum degree required by the vacuum equipment is 10 -3 Pa, the vacuum impregnation time was 20 minutes, and finally after drying at 130°C, the vacuum impregnation pretreated Tangdao brick recycled material was obtained; Step 3: weigh the raw materials according to the above ratio; Step 4: Place the fine powder of various raw materials, dispersant and thickener in a ball mill and mix for 5 hours to obtain a premixed powder; Step 5: Place the premixed powder and the vacuum impregnation pretreated recycled brick material in a high-powered mixer and stir for 10 minutes, then add the binder to obtain the high-temperature refractory mud material.

[0024] The high-temperature refractory clay prepared as above is used in the refractory gap of the mosaic sizing nozzle and the refractory gap between the nozzle seat brick and the nozzle, and its linear change rate within 1200-1600℃ is 1%-4%. When it is higher than 1400℃, the mullite content is greater than 80%. Example

[0025] The present embodiment provides a high-temperature refractory mortar with controllable expansion, comprising the following components: 60wt·% of recycled bricks after vacuum impregnation treatment, 28wt·% of raw mullite, 4wt·% of Guangxi mud, 8wt·% of aluminum waste, the total amount of the above raw materials is 100wt·%, and 0.5wt·% of a dispersant, 0.5wt·% of a thickener and 4wt·% of a binder are added to the total amount of the above raw materials; The Al2O3 of the recycled bricks treated by vacuum impregnation is greater than 70wt·%, and the mullite phase content is greater than 90wt·%; and the mixture is a mixture of 1-0.5mm and 0.5-0.2mm particles with a specific gravity of 1:2. The content of Al2O3 in mullite sand is 48wt·%, the content of SiO2 is 52wt·%, the content of mullite is more than 65wt·%, the content of cristobalite is 13wt·%, and the particle size is 200 mesh; Aluminum scrap is solid waste generated during the smelting process of aluminum metal, with Al2O3 content > 65wt·%, aluminum metal content < 4wt·%, and particle size D50 < 0.088μm; Guangxi mud has an Al2O3 content of >20wt·%, a plasticity index of >30, and a particle size of 200 mesh; The dispersant is a mixture of water-soluble sodium ammonium acrylate and triethylhexyl phosphoric acid; the thickener is one or two of sodium carboxymethyl cellulose; and the binder is potassium water glass.

[0026] The present embodiment also provides a method for preparing a high-temperature refractory clay with controllable expansion, characterized in that it specifically comprises the following steps: The first step is to crush, screen and magnetically separate the selected used soup duct bricks to obtain recycled soup duct bricks of different particle sizes; The second step is to use vacuum impregnation method to treat the recycled materials of Tangdao bricks. The impregnation liquid is made of mullite with a solid content of 65wt·% and the vacuum degree required by the vacuum equipment is 10 -3Pa, the vacuum impregnation time is 30 minutes, and finally after drying at 150°C, the vacuum impregnation pretreated Tangdao brick recycled material is obtained; Step 3: weigh the raw materials according to the above ratio; Step 4: Place the fine powder of various raw materials, dispersant and thickener in a ball mill and mix for 5 hours to obtain a premixed powder; Step 5: Place the premixed powder and the vacuum impregnation pretreated recycled brick material in a high-powered mixer and stir for 15 minutes, then add the binder to obtain the high-temperature refractory mud material.

[0027] The mullite content of the high-temperature refractory mud prepared above after heat treatment at 1600°C is about 86wt·%, and the linear change rate is 2.0%. Its use environment is the refractory mud joint between the tundish water nozzle and the seat brick. Example

[0028] The present embodiment provides a high-temperature refractory mud with controllable expansion, comprising the following components: 60wt·% of recycled Tangdao brick after vacuum impregnation treatment, 30wt·% of mullite raw material, 5wt·% of Guangxi mud, 5wt·% of aluminum waste, the total amount of the above raw materials is 100wt·%, and 1wt·% of the total amount of the above raw materials, 0.8wt·% of the thickener and 6wt·% of the binder are added; The Al2O3 of the recycled bricks treated by vacuum impregnation is greater than 70wt·%, and the mullite phase content is greater than 90wt·%; the mixture is a mixture of 1-0.5mm and 0.5-0.2mm particles with a specific gravity of 1:2; The content of Al2O3 in mullite sand is 40wt·%, the content of SiO2 is 60wt·%, the content of mullite is more than 65wt·%, the content of cristobalite is 20wt·%, and the particle size is 200 mesh; Aluminum scrap is solid waste generated during the smelting process of aluminum metal, with Al2O3 content > 65wt·%, aluminum metal content < 4wt·%, and particle size D50 < 0.088μm; Guangxi mud has an Al2O3 content of >20wt·%, a plasticity index of >30, and a particle size of 200 mesh; The dispersant is triethylhexyl phosphoric acid; the thickener is gelatin; and the binder is potassium water glass.

[0029] The present embodiment also provides a method for preparing a high-temperature refractory clay with controllable expansion, which is characterized in that it specifically comprises the following steps: The first step is to crush, screen and magnetically separate the selected used soup duct bricks to obtain recycled soup duct bricks of different particle sizes; The second step is to use vacuum impregnation method to treat the recycled materials of Tangdao bricks. The impregnation liquid is made of mullite with a solid content of 85wt·% and the vacuum degree required by the vacuum equipment is 10-3 Pa, the vacuum impregnation time was 30 minutes, and finally after drying at 160°C, the vacuum impregnation pretreated Tangdao brick recycled material was obtained; Step 3: weigh the raw materials according to the above ratio; Step 4: Place the fine powder of various raw materials, dispersant and thickener in a ball mill and mix for 5 hours to obtain a premixed powder; Step 5: Place the premixed powder and the vacuum impregnation pretreated Tangdao brick recycled material in a high-powered mixer and stir for 20 minutes, then add the binder to obtain the high-temperature refractory mud.

[0030] The mullite content of the high-temperature refractory mud prepared above after heat treatment at 1500°C is about 83wt·%, and the linear change rate is 2.6%. Its use environment is the refractory mud joint between the tundish water inlet and the seat brick.

[0031] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A high-temperature refractory clay with controllable expansion, characterized in that: The invention comprises the following components: 30-70wt% of recycled Tangdao bricks after vacuum impregnation treatment, 10-60wt% of raw mullite, 1-6wt% of Guangxi mud, 3-9wt% of aluminum waste, and the total amount of the above raw materials is 100wt%. Meanwhile, 0.1-1wt% of dispersant, 0.1-0.8wt% of thickener and 2-6wt% of binder are added to the total amount of the above raw materials.

2. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The vacuum impregnation treated soup ditch brick recycled material is obtained by a series of treatment processes such as crushing, screening, magnetic separation, vacuum impregnation, drying and the like of used soup ditch bricks.

3. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The Al2O3 content of the vacuum impregnated recycled brick material is greater than 70wt·%, and the mullite phase content is greater than 90wt·%; the particle size is 1-0.5mm and 0.5-0.2mm, and the specific gravity is 1:

2.

4. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The mullite sand has an Al2O3 content of 30-48wt·%, an SiO2 content of 40-60wt·%, a mullite content of more than 65wt·%, a cristobalite content of 10-20wt·%, and a particle size of 200-325 meshes.

5. The high-temperature refractory clay with controllable expansion according to claim 2, characterized in that: The impregnation liquid required for the vacuum impregnation treatment of the recycled materials of the soup road brick is a mullite material with a solid content of 30-85wt·%, and the vacuum degree required by the vacuum equipment is 10 -3 -10 -5 Pa, vacuum impregnation time is 5-30 minutes.

6. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The aluminum scrap is solid waste generated during the smelting process of metallic aluminum, and its Al2O3 content is greater than 65wt·%, the content of metallic aluminum is less than 4wt·%, and the particle size is D50 less than 0.088μm.

7. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The Guangxi mud has an Al2O3 content of more than 20wt·%, a plasticity index of more than 30, and a particle size of 200-300 meshes.

8. The high-temperature refractory clay with controllable expansion according to claim 1, characterized in that: The dispersant is one or both of water-soluble sodium ammonium acrylate or triethylhexyl phosphate; the thickener is one or both of gelatin or sodium carboxymethyl cellulose; and the binder is one or both of potassium water glass or aluminum dihydrogen phosphate.

9. A method for preparing a high-temperature refractory clay with controllable expansion according to any one of claims 1 to 8, characterized in that: Specifically include the following steps: The first step is to crush, screen and magnetically separate the selected used soup duct bricks to obtain recycled soup duct bricks of different particle sizes; The second step is to use vacuum impregnation method to treat the recycled materials of Tangdao bricks. The impregnation liquid is mullite sand with a solid content of 30-85wt·% and the vacuum degree required by the vacuum equipment is 10 -3 -10 -5 Pa, the vacuum impregnation time is 5-30 minutes, and finally after drying at 110-180°C, the vacuum impregnation pretreated Tangdao brick recycled material is obtained; Step 3: weigh the raw materials according to the fixed ratio; Step 4: Place the fine powder of various raw materials, dispersant and thickener in a ball mill and mix for 2-6 hours to obtain a premixed powder; Step 5: Place the premixed powder and the vacuum impregnation pretreated recycled brick material in a high-powered mixer and stir for 5-20 minutes, then add the binder to obtain the high-temperature refractory mud material.

10. A high-temperature refractory clay with controllable expansion and a preparation method thereof according to claims 1 to 9, characterized in that: The high-temperature refractory clay produced is used in the refractory gaps of the inlaid sizing nozzles and the refractory gaps between the nozzle seat brick and the nozzle, and its linear change rate within 1200-1600°C is 0.5%-5%. When the temperature is higher than 1400°C, the mullite content is greater than 80%.

Citation Information

Patent Citations

  • Anti-seepage steel environment-friendly tundish fire clay, preparation method and construction method

    CN112374874A

  • Micro-expansion carbon-containing refractory mortar for sliding nozzle, and production method thereof

    CN113956056A

  • Micro-expansion high-strength wear-resistant zirconium-inlaid fire clay and preparation method thereof

    CN117800715A

  • Production of casting material using alumina based refractory waste material

    JP1998130066A