CVI (Chemical Vapor Infiltration) densification method for thick three-dimensional needled component

By segmenting and stacking the thick three-dimensional needle-punching members, and using CVI method and ceramic matrix composite fasteners, the problems of slow density, difficult density and uneven density are solved, and the density uniformity and mechanical properties of the components are achieved Improvement.

CN118930299APending Publication Date: 2024-11-12XIAN XINGUI CERAMIC COMPOSITE MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411033586.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Thick size three-dimensional needle-punching members have problems such as slow density, difficult density, uneven density during the densification process in the CVI method, and their mechanical properties are low.

Method used

The prefabricated body of the thick three-dimensional needle-punched member is divided into main body flat plate blanks with ≤12mm, and the breathable holes are prepared, and the density is carried out by chemical vapor deposition CVI method, followed by stacking assembly and riveting treatment, using ceramic matrix composite material Fastener connectors are integrally connected and processed.

Benefits of technology

The density uniformity and mechanical properties of thick three-dimensional needle-punched members are improved, and the problems of slow density, difficult density and uneven density are solved. The prepared components have excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930299A_ABST
    Figure CN118930299A_ABST
Patent Text Reader

Abstract

The invention relates to a CVI (Chemical Vapor Infiltration) densification method for a thick three-dimensional needling component, belongs to the technical field of composite material densification, and solves the technical problems of slow densification, difficult densification and non-uniform densification of the thick three-dimensional needling component. Carrying out CVI densification treatment on the main body flat plate blank; laminating and assembling; and a rivet welding treatment step. The CVI densification method is used for chemical vapor deposition densification of the thick three-dimensional needling component, a solution thought is provided for preparation of various special-shaped thick three-dimensional needling components, and the prepared thick three-dimensional needling component has the advantages of being uniform in density and excellent in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material densification, and in particular relates to a CVI densification method for thick-sized three-dimensional needle-punched components. Background Art

[0002] Ceramic matrix composites are a new type of thermal structural / functional integrated material that combines the performance advantages of metal materials, ceramic materials and carbon materials. They overcome the shortcomings of metal materials such as low temperature resistance and high density, ceramic materials such as high brittleness and poor reliability, and carbon materials such as poor oxidation resistance and low strength. They have the characteristics of high temperature resistance, low density, high specific strength, high specific modulus, oxidation resistance, ablation resistance, insensitivity to cracks, and no catastrophic damage. They are widely used in the aerospace field. Thick-sized three-dimensional needle-punched flat plate components are widely used, but for thick plate components (≥12mm), the components prepared by the CVI method often have problems such as slow densification, difficult densification, and uneven densification. The mechanical properties of the components that have been modified will be significantly lower than those prepared by the CVI method. Therefore, it is particularly important to study and solve the CVI densification problem of thick-sized three-dimensional needle-punched components. Summary of the invention

[0003] In order to overcome the problems of slow densification, difficult densification and uneven densification of thick-sized three-dimensional needle-punched components, the present invention proposes a CVI densification method for thick-sized three-dimensional needle-punched components.

[0004] The technical solution adopted by the present invention to solve the technical problem is:

[0005] A CVI densification method for thick-sized three-dimensional needle-punched components comprises the following steps:

[0006] Step S1: splitting the preform blank and preparing the vent holes

[0007] The thick three-dimensional needle-punched component preform blank is divided into several main flat plate blanks with a thickness of ≤12mm. The main flat plate blank is in a rectangular shape. Air holes are prepared on the main flat plate blank. The air holes are used to increase air permeability and fastener installation during the CVI process to obtain a main flat plate blank with air holes.

[0008] Step S2: CVI densification treatment of the main flat plate blank

[0009] The main plate is obtained by densifying the main plate blank with air permeable holes using a chemical vapor deposition (CVI) method.

[0010] Step S3: stacking assembly

[0011] On the basis of the vent hole, a fastener mounting hole is processed, and the fastener mounting hole is used for mounting the fastener.

[0012] The main plates are connected and fastened together by fasteners to obtain a laminated main plate component in which the main plates are laminated and assembled together.

[0013] Step S4: Riveting and welding

[0014] The CVI method is adopted to carry out CVI deposition on the laminated main plate component, and the component is mechanically processed according to the requirements of the external structure size to obtain a densified thick-size three-dimensional needle-punched component which is riveted and welded together.

[0015] In the above-mentioned CVI densification method, the main flat plate blank is a C / SiC composite material, and a process table and a processing reference hole are provided at both ends. The process table is used for installing the first reinforcement box body and the second reinforcement box body, and the processing reference hole is used for positioning and alignment.

[0016] In the above-mentioned CVI densification method, the thick-sized three-dimensional needle-punched component preform blank can be a flat component blank or a special-shaped component blank.

[0017] In the above-mentioned CVI densification method, the center of the air vent coincides with the center of the fastener mounting hole, and the diameter of the air vent is less than or equal to the diameter of the fastener mounting hole.

[0018] In the above-mentioned CVI densification method, the diameter of the ventilation hole is at least 0.5 mm smaller than the diameter of the fastener installation hole.

[0019] In the above-mentioned CVI densification method, the step S2 of CVI densification treatment of the main flat plate blank further comprises:

[0020] The main flat blank CVI density is 1.2-1.3 g / cm 3 , rough machining of components; CVI to density of 1.4-1.5g / cm 3 , the components are semi-finished for the first time to prepare φ2 air holes; CVI to a density of 1.6-1.7 g / cm 3 , the component is semi-finished for the second time, and the air hole is expanded to φ2.5; CVI is adjusted to a density of 1.7-1.8g / cm 3 , the component is semi-finished for the third time, and the air hole is expanded to φ3; CVI is adjusted to a density of 1.8-1.9 g / cm 3 , finish machining the components;

[0021] Before rough machining, the blank component should ensure that the distance between the outer surface of the part and the final part thickness is ≥2mm;

[0022] The minimum distance between the outer surface of the main plate after rough machining and the final part is 1.5mm, and the minimum distance between the side wall and the final part is 1.5mm;

[0023] In the first semi-finishing, all outer surfaces of the part are machined off by 0.5mm on the basis of rough machining, and the air holes are machined to the end; in the second semi-finishing, all outer surfaces of the part are machined off by 0.5mm on the basis of the first semi-finishing, and the air holes are expanded; in the third semi-finishing, all outer surfaces of the part are machined off by 0.3mm on the basis of the second semi-finishing, and the air holes are expanded; in the finishing, all outer surfaces of the part are machined off by 0.2mm on the basis of the second semi-finishing, and the air holes are machined to the size required for the connection of the connector.

[0024] In the above CVI densification method, the main body plate includes a first main body plate, a second main body plate, a third main body plate, and a fourth main body plate, and the first main body plate, the second main body plate, the third main body plate, and the fourth main body plate are placed in sequence.

[0025] In the above-mentioned CVI densification method, the fasteners are ceramic-based composite materials, including pins, screws, countersunk nuts, and studs; the pins, screws, countersunk nuts, and studs connect the first reinforcement box body, the second reinforcement box body, and the main plate into a whole.

[0026] In the above-mentioned CVI densification method, the fastener is a ceramic matrix composite component, including a pin, a screw, a countersunk nut, and a stud; the pin, the screw, the countersunk nut, and the stud connect the first reinforcement box body, the second reinforcement box body, and the main plate into a whole;

[0027] The fastener mounting holes include pin holes, screw holes, countersunk nut holes, and stud holes. The pin holes are used for mounting pins, the screw holes are used for mounting screws, the countersunk nut holes are used for mounting countersunk nuts, and the stud holes are used for mounting studs.

[0028] In the above-mentioned CVI densification method, the first reinforcement box body and the second reinforcement box body are 2D components, which are respectively located at two ends of the main plate, and are provided with U-shaped openings to clamp the main plate.

[0029] In the above-mentioned CVI densification method, the spacing between the air holes on the periphery of the laminated main plate component is 10 to 15 mm.

[0030] The beneficial effects of the present invention are:

[0031] A CVI densification method for thick-sized three-dimensional needle-punched components solves the problems of slow densification, difficult densification and uneven densification of thick-sized three-dimensional needle-punched flat plates; the thick-sized three-dimensional needle-punched components prepared using the method of the invention have the characteristics of uniform density and excellent mechanical properties.

[0032] A CVI densification method for thick-sized three-dimensional needle-punched components provides a solution for the preparation of various special-shaped thick-sized three-dimensional needle-punched components. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of a thick three-dimensional needle-punched component according to an embodiment of the present invention;

[0034] Figure 2 Schematic diagram of the composition of a thick three-dimensional needle-punched component according to an embodiment of the present invention;

[0035] Figure 3 This is a flow chart of the preparation of the main plate of the embodiment of the present invention;

[0036] Figure 4 It is a schematic diagram of the composition of the first to fourth main plates;

[0037] Figure 5 is a schematic diagram of the first reinforcement box structure;

[0038] Figure 6 Schematic diagram of the second reinforcement box structure.

[0039] Figure numerals: 1. first main body plate, 2. second main body plate, 3. third main body plate, 4. fourth main body plate, 5. first reinforcement box body, 6. second reinforcement box body, 7. pin, 8. screw, 9. countersunk nut, 10. stud. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] Embodiment 1

[0042] A CVI densification method for thick-sized three-dimensional needle-punched flat components divides the thick-sized three-dimensional needle-punched flat component into a plurality of main flat parts with a thickness of ≤12 mm along the thickness direction, and connects and fastens the divided main flat parts using a connection method of composite material fasteners to achieve a thin-walled design of the thick-sized three-dimensional needle-punched flat component.

[0043] The main plate parts after segmentation can be flat plates or special-shaped plates.

[0044] The fasteners used for connecting and fastening the main plate are pins, screws, countersunk screws, countersunk nuts and other ceramic-based composite material connecting parts.

[0045] During the CVI preparation process of the divided main plate, in order to make the components more compact, ventilation holes are prefabricated in advance using the holes for subsequent fastener connections during the parts compaction process. The center of the ventilation hole coincides with the center of the fastener, and the diameter of the ventilation hole is at least 0.5 mm smaller than the diameter of the fastener.

[0046] During the preparation process of the main flat plate parts after segmentation, allowance must be made, and processing heads and processing reference holes must be set at both ends of the parts so that the components can be quickly aligned and finely processed during the subsequent connection and assembly process.

[0047] A CVI densification method for a thick three-dimensional needle-punched flat plate. The divided main plates are assembled in a stacking manner. The main plates are named from bottom to top as a first main plate 1, a second main plate 2, a third main plate 3, a fourth main plate 4, ..., and the specific assembly steps are as follows:

[0048] 1) The bottom surface of the first main body plate 1 is finely processed with allowance, and the upper surface of the first main body plate 1 is processed to the final part state based on the processed bottom surface of the first main body plate 1;

[0049] 2) Using the top surface of the second main body plate 2 as a reference, the bottom surface of the second main body plate 2 is processed to the final part state;

[0050] 3) Positioning is performed using the process head reference holes on the first main plate 1 and the second main plate 2, and the bottom surface of the second main plate 2 is stacked on the upper surface of the first main plate 1;

[0051] 4) Processing the first main plate 1 and the second main plate 2 stacked together, wherein only the upper surface of the main plate 2 is processed;

[0052] 5) Using the top surface of the third main body plate 3 as a reference, process the bottom surface of the third main body plate 3 to the final part state;

[0053] 6) Positioning with the reference hole, the bottom surface of the third main plate 3 is stacked on the upper surface of the second main plate 2, so that the first main plate 1, the second main plate 2, and the third main plate 3 become a whole;

[0054] 7) Processing the first main plate 1, the second main plate 2, and the third main plate 3 stacked together, and processing only the upper surface of the third main plate 3;

[0055] 8) Repeat the above steps to achieve stacking of the fourth main body plate 4, the fifth main body plate, the sixth main body plate, etc.;

[0056] 9) Prepare fastening and connection holes for the stacked main plates. The hole positions must be consistent with the pin holes made in the early stage.

[0057] 10) Fasten and connect the stacked main panels;

[0058] 11) CVI deposition is performed on the connected components, and “riveting” is performed on the fasteners and the main plate;

[0059] 12) The outer shape of the main plate is processed uniformly to obtain the final thick-sized three-dimensional needle-punched plate component.

[0060] Embodiment 2

[0061] Take the CVI densification of a three-dimensional needle-punched preform with a specification of 296*81.5*48mm as an example. Figure 1 shown.

[0062] 1) According to the product structure and characteristics, the products are divided into the following forms, such as Figure 2 As shown: it includes a first main body plate 1, a second main body plate 2, a third main body plate 3, a fourth main body plate 4, a first reinforcement box body 5, a second reinforcement box body 6, a pin 7, a screw 8, a countersunk nut 9, and a stud 10. The second main body plate 2 is laid flat on the first main body plate 1, the third main body plate 3 is laid flat on the second main body plate 2, and the fourth main body plate 4 is laid flat on the third main body plate 3. The first main body plate 1, the second main body plate 2, the third main body plate 3, and the fourth main body plate 4 are clamped through the U-shaped opening of the first reinforcement box body 5 and the second reinforcement box body 6, and the above parts are connected into a whole by using pins 7, screws 8, countersunk nuts 9, and studs 10 to form a final laminated ceramic matrix composite main plate component.

[0063] 2) All parts of this product are made of C / SiC composite materials. The first reinforcement box 5, the second reinforcement box 6, and the pin 7 are 2D components; the rest are 3DN components.

[0064] 3) The main structure of the product is composed of four stacked flat plates, each of which has a maximum thickness of 12 mm and is a special-shaped component made from a three-dimensional needle-punched preform. During the deposition process, each plate is a rectangular component with a process table and processing reference holes at both ends. The arc-shaped surface is not processed during the deposition process.

[0065] 4) The first reinforcement box body 5 and the second reinforcement box body 6 are made of a two-dimensional laminated preform with a wall thickness of 3 mm.

[0066] 5) The preparation process of the main plate is as follows Figure 3 A preform blank with a wall thickness of 14 mm was prepared by chemical vapor deposition to a density of 1.2 to 1.3 g / cm 3 The components are rough-machined to ensure that the distance between the outer surface of the parts and the final thickness of the parts is 1.5 mm after rough machining; chemical vapor deposition is performed after rough machining until the density reaches 1.4-1.5 g / cm 3 After the rough machining, the parts are first finished, all the outer surfaces of the parts are machined off by 0.5mm, and φ2 air holes are made; after the first semi-finishing, chemical vapor deposition is carried out until the density reaches 1.6-1.7g / cm3 The second semi-finishing is performed on the parts based on the first semi-finishing. All the outer surfaces of the parts are machined down by 0.5mm, and the air holes are expanded to φ2.5. After the second semi-finishing, chemical vapor deposition is performed until the density reaches 1.7-1.8g / cm 3 On the basis of the second semi-finishing, the parts are semi-finished for the third time, all the outer surfaces of the parts are machined off by 0.3mm, and the vent holes are expanded to φ3; after the third semi-finishing, chemical vapor deposition is carried out until the density reaches 1.8-1.9g / cm 3 When the thickness of all outer surfaces of the parts is reduced by 0.2 mm on the basis of the third semi-finishing, the main flat plate parts to be processed and assembled are formed after CVI deposition.

[0067] 7) The position of the vent holes coincides with the position of all pin holes and screw holes for the final connection of the product. The vent holes on the periphery of the parts are arranged according to a hole spacing of 10 to 15 mm.

[0068] 8) After the main plate is prepared, the main plate is assembled by a stacking method, as follows:

[0069] a. Taking the bottom surface of the first main body plate 1 as a reference, the upper surface of the first main body plate 1 is processed to the final part state;

[0070] b. Using the top surface of the second main body plate 2 as a reference, process the bottom surface of the second main body plate 2 to the final part state;

[0071] c. Positioning by using the reference hole, the bottom surface of the second main body plate 2 is placed on the upper surface of the first main body plate 1;

[0072] d. Processing the first main plate 1 and the second main plate 2 stacked together, and processing only the upper surface of the second main plate 2;

[0073] e. Using the top surface of the third main body plate 3 as a reference, process the bottom surface of the third main body plate 3 to the final part state;

[0074] f. Positioning by using the reference hole, the bottom surface of the third main plate 3 is stacked on the upper surface of the second main plate 2, so that the first main plate 1, the second main plate 2, and the third main plate 3 become a whole;

[0075] g. Processing the first main plate 1, the second main plate 2, and the third main plate 3 stacked together, and processing only the upper surface of the third main plate 3;

[0076] h. Using the top surface of the fourth main body plate 4 as a reference, process the bottom surface of the fourth main body plate 4 to the final part state;

[0077] i. Positioning with the reference hole, the bottom surface of the fourth main plate 4 is stacked on the upper surface of the third main plate 3, so that the first main plate 1, the second main plate 2, the third main plate 3, and the fourth main plate 4 become a whole;

[0078] j. Process all the shapes of the parts to obtain the final main flat plate component.

[0079] 9) Install the first reinforcement box body 5 and the second reinforcement box body 6, make fastening holes and connection holes, connect all components into a whole, and obtain a densified three-dimensional needle-punched preform main plate component.

Claims

1. A CVI densification method for thick-sized three-dimensional needle-punched components, characterized in that: The following steps are involved: Step S1, splitting the preform blank and preparing the vent holes: The thick three-dimensional needle-punched component preform blank is divided into several main flat blanks with a thickness of ≤12 mm. The main flat blank is in a rectangular shape. Air holes are prepared on the main flat blank. The air holes are used to increase air permeability and fastener installation during the CVI process to obtain a main flat blank with air holes; Step S2, CVI densification treatment of the main flat plate blank: The main plate blank with air permeable holes is densified by using a chemical vapor deposition (CVI) method to obtain the main plate; Step S3, stacking assembly: On the basis of the vent hole, a fastener installation hole is processed, and the fastener installation hole is used for installing the fastener; The main plates are connected and fastened together by fasteners to obtain a laminated main plate component in which the main plates are laminated and assembled together; Step S4, riveting and welding: The CVI method is adopted to carry out CVI deposition on the laminated main flat plate, and mechanical processing is carried out according to the requirements of the external structure size to obtain a densified thick-size three-dimensional needle-punched component which is riveted and welded together.

2. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The main flat plate blank is made of C / SiC composite material, and is provided with a process table and a processing reference hole at both ends. The process table is used for processing and clamping, and the processing reference hole is used for positioning and alignment.

3. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The thick-size three-dimensional needle-punched component preform blank may be a flat component blank or a special-shaped component blank.

4. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The center of the air vent coincides with the center of the fastener mounting hole.

5. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 4, characterized in that: The diameter of the ventilation hole is at least 0.5 mm smaller than the diameter of the fastener installation hole, and the minimum diameter of the ventilation hole should be greater than 2 mm.

6. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The step S2 of subjecting the flat plate blank to CVI densification treatment further comprises: The main flat blank CVI density is 1.2-1.3 g / cm 3 , rough machining of components; CVI to density of 1.4-1.5g / cm 3 , the components are semi-finished for the first time to prepare φ2 air holes; CVI to a density of 1.6-1.7 g / cm 3 , the component is semi-finished for the second time, and the air hole is expanded to φ2.5; CVI is adjusted to a density of 1.7-1.8g / cm 3 , the component is semi-finished for the third time, and the air hole is expanded to φ3; CVI is adjusted to a density of 1.8-1.9 g / cm 3 , finish machining the components; Before rough machining, the blank component should ensure that the distance between the outer surface of the part and the final part thickness is ≥2mm; The minimum distance between the outer surface of the main plate after rough machining and the final part is 1.5mm, and the minimum distance between the side wall and the final part is 1.5mm; The first semi-finishing is to machine 0.5mm off all the outer surfaces of the parts on the basis of rough machining, and to machine the vent holes; the second semi-finishing is to machine 0.5mm off all the outer surfaces of the parts on the basis of the first semi-finishing, and to expand the vent holes; the third semi-finishing is to machine 0.3mm off all the outer surfaces of the parts on the basis of the second semi-finishing, and to expand the vent holes; the finishing is to machine 0.2mm off all the outer surfaces of the parts on the basis of the second semi-finishing. And process the vent holes to the size required for the connectors.

7. The CVI densification method of thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The main body plate comprises a first main body plate (1), a second main body plate (2), a third main body plate (3), and a fourth main body plate (4), wherein the first main body plate (1), the second main body plate (2), the third main body plate (3), and the fourth main body plate (4) are placed in sequence.

8. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The fastener is a ceramic matrix composite material component, comprising a pin (7), a screw (8), a countersunk nut (9), and a stud (10); the pin (7), the screw (8), the countersunk nut (9), and the stud (10) connect the first reinforcement box body (5), the second reinforcement box body (6), and the main plate into a whole; The fastener installation holes include pin holes, screw holes, countersunk nut holes, and stud holes. The pin holes are used for installing pins (7), the screw holes are used for installing screws (8), the countersunk nut holes are used for installing countersunk nuts (9), and the stud holes are used for installing studs (10).

9. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 8, characterized in that: The first reinforcement box body (5) and the second reinforcement box body (6) are 2D components, and are respectively located at two ends of the main plate. Set up a U-shaped opening to clamp the main plate.

10. The CVI densification method for thick-sized three-dimensional needle-punched components according to claim 1, characterized in that: The spacing between the air holes on the periphery of the laminated main plate component is 10 to 15 mm.

Citation Information

Patent Citations

  • Preparation method of SiCw directional high toughness thick-wall ceramic matrix composite material

    CN109721376A

  • CVI densification method for large-wall-thickness ceramic matrix composite part

    CN111170751A

  • Labyrinth cavity component of ceramic matrix composite product and flow guide deposition method

    CN117104493A

  • Carbon-carbon composite material spliced thermal insulation cylinder and production process thereof

    CN117989417A