Tungsten carbide embedded carbon nano tube block composite material as well as preparation method and application thereof
By growing tungsten carbide nanowires in the limited domain of carbon nanotubes and using discharge plasma sintering technology, the problem of preparation and assembly of carbon nanotube bulk composites has been solved, and the preparation of high-performance carbon nanotube bulk composites has been realized, which has significantly improved the Mechanical properties of materials.
Patent Information
- Application Number
- CN202411199769.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The prior art When carbon nanotubes are assembled into macroscopic composites across scales, the agglomeration and interface effects of carbon nanotubes are weak, which limits the performance of their excellent performance. In particular, there are fewer technologies for the preparation and assembly of carbon nanotubes, which are difficult to achieve. High-performance carbon nanotube-based composite materials.
The carbon nanotubes are mixed, filtered and dried with phosphotungstic acid, and reduced treatment is performed to limit the domain growth of tungsten carbide nanowires, and then the tungsten carbide embedded carbon nanotube bulk composite material is prepared by discharge plasma sintering technology.
Macro-preparation of 100 grams of tungsten carbide embedded carbon nanotube powder was achieved, and a new light specific gravity carbon nanotube bulk composite material with high temperature resistance and excellent mechanical properties was obtained, which significantly improved the hardness and elastic modulus of the material.
Smart Images

Figure CN118930301A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a tungsten carbide embedded carbon nanotube bulk composite material and a preparation method and application thereof, belonging to the technical field of material preparation. Background Art
[0002] As a member of the carbon material family, carbon nanotubes have great potential in the development of lightweight, high-performance composite materials in aerospace and other fields due to their outstanding characteristics such as low density, excellent mechanical properties, high thermal conductivity and unique electrical properties. However, when carbon nanotubes with excellent performance are assembled into macroscopic composite materials across scales, problems such as carbon nanotube agglomeration and weak interface interaction limit the performance of carbon nanotubes, resulting in a significant reduction in the performance of macroscopic carbon nanotube-based composite materials.
[0003] It is worth noting that the hollow tube cavity in the carbon nanotube is one of its most basic structural units. The cavity has a high specific surface area and internal space, which can provide good carrying and storage conditions for various molecules, ions and other substances. Carbon nanotubes can react through the nanospace of the hollow tube, thereby confining the growth of guest materials. For this reason, if high-temperature resistant nanomaterials can be filled and grown in carbon nanotubes and assembled into macroscopic bulk materials, it will be expected to be applied in major national high-tech equipment such as aerospace.
[0004] Currently, most of the assembly technologies for carbon nanotube macrostructures are concentrated on carbon nanotube fibers and carbon nanotube films. There are few articles and patent reports on carbon nanotube blocks, and there are no patent articles on the large-scale preparation of embedded carbon nanotube powders and their block assembly. Summary of the invention
[0005] The main purpose of the present invention is to provide a tungsten carbide embedded carbon nanotube bulk composite material and a preparation method thereof, so as to overcome the deficiencies in the prior art.
[0006] Another object of the present invention is to provide an application of the tungsten carbide embedded carbon nanotube bulk composite material.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] The embodiment of the present invention provides a method for preparing a tungsten carbide embedded carbon nanotube bulk composite material, which comprises:
[0009] Mixing carbon nanotube slurry and phosphotungstic acid, filtering, and drying to obtain phosphotungstic acid embedded carbon nanotube powder;
[0010] The phosphotungstic acid embedded carbon nanotube powder is subjected to reduction treatment, so that tungsten carbide nanowires are confined and filled in the carbon nanotubes to grow, thereby obtaining tungsten carbide embedded carbon nanotube powder;
[0011] The tungsten carbide embedded carbon nanotube powder is subjected to spark plasma sintering to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0012] In some embodiments, the preparation method comprises:
[0013] Placing the tungsten carbide embedded carbon nanotube powder in a graphite mold, and then placing it in a spark plasma sintering system, compacting the tungsten carbide embedded carbon nanotube powder, and evacuating the spark plasma sintering system;
[0014] The graphite mold is heated, and pressure is applied to both ends of the compacted tungsten carbide embedded carbon nanotube powder, thereby performing the spark plasma sintering.
[0015] The embodiment of the present invention also provides a tungsten carbide embedded carbon nanotube bulk composite material prepared by the above preparation method.
[0016] The embodiment of the present invention also provides the application of the aforementioned tungsten carbide embedded carbon nanotube bulk composite material in the aerospace field.
[0017] Compared with the prior art, the advantages of the present invention are at least:
[0018] The preparation method provided by the present invention utilizes carbon nanotubes as a template to achieve large-scale preparation of 100-gram-level tungsten carbide embedded carbon nanotube powders, and obtains tungsten carbide embedded carbon nanotube bulk composite materials through spark plasma sintering technology. The preparation process is fast and convenient, and a new type of light specific gravity carbon nanotube bulk composite material with high temperature resistance and excellent mechanical properties is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 This is a process flow chart of preparing a bulk composite material of tungsten carbide embedded with carbon nanotubes in a typical embodiment of the present invention;
[0021] Figure 2 This is a transmission electron microscope image of the tungsten carbide embedded carbon nanotube powder obtained in step (1) of Example 1 of the present invention;
[0022] Figure 3 This is a physical picture of the tungsten carbide embedded carbon nanotube bulk composite material obtained in step (2) of Example 1 of the present invention;
[0023] Figure 4 This is a cross-sectional scanning electron microscope image of the tungsten carbide embedded carbon nanotube bulk composite material obtained in step (2) of Example 1 of the present invention;
[0024] Figure 5 XRD patterns of the tungsten carbide embedded carbon nanotube powder and the tungsten carbide embedded carbon nanotube bulk composite material obtained in Example 1 of the present invention;
[0025] Figure 6 It is an instrumented micron indentation load-displacement curve diagram of carbon nanotubes and the tungsten carbide embedded carbon nanotube bulk composite material obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution mainly provides a method for preparing a tungsten carbide embedded carbon nanotube bulk composite material, uses carbon nanotubes as a template to achieve large-scale preparation of tungsten carbide embedded carbon nanotube powder, and obtains the tungsten carbide embedded carbon nanotube bulk composite material by spark plasma sintering technology.
[0027] The technical solution, its implementation process and principle are further explained as follows. However, it should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described in the following (embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.
[0028] As one aspect of the technical solution of the present invention, a method for preparing a tungsten carbide embedded carbon nanotube bulk composite material involves:
[0029] Mixing carbon nanotube slurry and phosphotungstic acid, filtering, and drying to obtain phosphotungstic acid embedded carbon nanotube powder;
[0030] The phosphotungstic acid embedded carbon nanotube powder is subjected to reduction treatment, so that tungsten carbide nanowires are confined and filled in the carbon nanotubes to grow, thereby obtaining tungsten carbide embedded carbon nanotube powder;
[0031] The tungsten carbide embedded carbon nanotube powder is subjected to spark plasma sintering to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0032] In some specific embodiments, the preparation method includes: ultrasonically dispersing carbon nanotubes in water to obtain carbon nanotube slurry.
[0033] Furthermore, the mass fraction of the carbon nanotube slurry is 0.1-0.5%.
[0034] In some specific embodiments, the preparation method includes: adding phosphotungstic acid to carbon nanotube slurry, stirring and mixing, filtering the obtained mixed solution, ball milling after drying, and sieving powder to obtain phosphotungstic acid embedded carbon nanotube powder.
[0035] In some specific embodiments, the mass ratio of the phosphotungstic acid to the carbon nanotubes is 10:1 to 40:1.
[0036] Furthermore, the stirring time is 1 to 6 days.
[0037] Furthermore, the particle size of the mixed powder is 100 to 300 meshes.
[0038] In some specific embodiments, the preparation method includes: heating the phosphotungstic acid embedded carbon nanotube powder at 100-500°C for 4-10 hours, further drying the powder to remove bound water on the phosphotungstic acid, then heating to 600-950°C, and performing a reduction treatment in a reducing atmosphere for 1-5 hours to obtain tungsten carbide embedded carbon nanotube powder.
[0039] Furthermore, the reducing atmosphere includes a mixed atmosphere of hydrogen and an inert gas (such as argon).
[0040] Furthermore, the volume percentage of hydrogen in the mixed atmosphere is 20-40%.
[0041] In some specific embodiments, the diameter of the tungsten carbide nanowire is 0.5-4 nm.
[0042] In some specific embodiments, the content of phosphotungstic acid in the phosphotungstic acid embedded carbon nanotube powder is 20-50 wt %.
[0043] In some specific embodiments, the preparation method comprises:
[0044] Placing the tungsten carbide embedded carbon nanotube powder in a graphite mold, and then placing it in a spark plasma sintering system, compacting the tungsten carbide embedded carbon nanotube powder, and evacuating the spark plasma sintering system;
[0045] The graphite mold is heated, and pressure is applied to both ends of the compacted tungsten carbide embedded carbon nanotube powder, thereby performing the spark plasma sintering.
[0046] In some more preferred embodiments, the preparation method specifically includes: heating the graphite mold at a heating rate of 10 to 100°C / min to raise the temperature to 1000 to 1600°C, and applying a pressure of 20 to 60 MPa to both ends of the compacted tungsten carbide embedded carbon nanotube powder; and the spark plasma sintering time is 5 to 60 min.
[0047] Among them, for some more specific implementation plans, please refer to Figure 1 As shown, the steps of preparing the tungsten carbide embedded carbon nanotube bulk composite material of the present invention are as follows:
[0048] (1) Preparation of tungsten carbide embedded carbon nanotube powder
[0049] A. ultrasonically dispersing carbon nanotubes in water to prepare a carbon nanotube slurry having a mass fraction of 0.1 to 0.5% (e.g., 0.1%, 0.2%, 0.33%, 0.4%, 0.5%, etc.);
[0050] B. adding phosphotungstic acid powder to the carbon nanotube slurry, wherein the mass ratio of phosphotungstic acid to carbon nanotube is 10:1 to 40:1, for example, 10:1, 20:1, 30:1, 40:1, etc., and stirring with a stirrer for 1 to 6 days;
[0051] C. Pour the mixed solution obtained in step B into a suction filtration bottle, and filter and wash with deionized water until the pH value reaches 7;
[0052] D. drying the obtained powder in a drying oven at 10-100° C. / min, ball-milling the powder and sieving the powder to collect the powder with a particle size less than 300 mesh, preferably 100-300 mesh, for example, the powder may be 100 mesh, 200 mesh, 300 mesh, etc.;
[0053] E. Place the powder in a muffle furnace and keep it at a temperature of 100 to 500° C., for example, 100, 300, 500° C., etc. for 4 to 10 hours;
[0054] F. Keep the powder at 600-950°C, for example, 600, 700, 800, 950°C, under the condition of passing argon-hydrogen mixed gas (40% hydrogen) for 1-5 hours, for example, 1 hour, 3 hours, 5 hours, etc.
[0055] (2) Sintering of tungsten carbide embedded carbon nanotube powder
[0056] A. Place a layer of graphite paper on the bottom and sides of the graphite mold;
[0057] B. placing the ground powder into a cylindrical graphite mold with a sintering diameter of 50 mm, and then placing the mold into a spark plasma sintering system, compacting the mixed powder and evacuating the plasma sintering system;
[0058] C. heating the graphite mold to 1000-1600° C. at a heating rate of 10-100° C. / min, for example, 1000° C., 1300° C., 1600° C., etc., and applying a pressure of 20-60 MPa to both ends of the compacted powder material during the heating process, for example, 20 MPa, 40 MPa, 60 MPa, etc.;
[0059] D. The compacted powder is kept in an environment with a sintering temperature of 1000-1600°C and a sintering pressure of 20-60 MPa for 5-60 min, for example, 5 min, 10 min, 30 min, 60 min, etc.;
[0060] E. After sintering is completed, cool the sintering furnace to room temperature and take out the sample.
[0061] As another aspect of the technical solution of the present invention, it also relates to a tungsten carbide embedded carbon nanotube bulk composite material prepared by the aforementioned preparation method.
[0062] In some embodiments, the tungsten carbide embedded carbon nanotube bulk composite material has high strength and excellent mechanical properties. Specifically, the hardness of the composite material is 540 to 1000 MPa, and the elastic modulus is 4 to 10 GPa.
[0063] In summary, the present invention provides a carbon nanotube bulk composite material system, that is, the carbon nanotube bulk composite material is prepared by confined filling and growing tungsten carbide nanowires in carbon nanotubes, and then the obtained powder is subjected to spark plasma sintering, thereby realizing the assembly and preparation of a new type of embedded carbon nanotube macroscopic bulk composite material.
[0064] The present invention is the first to realize the large-scale preparation of tungsten carbide powder filled in carbon nanotubes, and realizes the powder assembly to prepare a new type of bulk material. The mechanical properties of the tungsten carbide embedded carbon nanotube bulk material prepared by the present invention are significantly better than those of the carbon nanotube bulk, and it is expected to be applied in major national high-tech equipment such as aerospace.
[0065] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on it. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or under the conditions recommended by the manufacturer.
[0066] Comparative Example 1
[0067] The carbon nanotubes were sintered in a spark plasma device with a heating rate of 50°C / min, a sintering pressure of 40 MPa, a sintering temperature of 1600°C, and a holding time of 10 min.
[0068] Example 1
[0069] (1) Add carbon nanotubes to deionized water and disperse them by ultrasonic to obtain a carbon nanotube slurry with a mass fraction of 0.33%, then add phosphotungstic acid to the carbon nanotube slurry and stir it in a stirrer for four days. The mass ratio of phosphotungstic acid to carbon nanotubes is 20:1. Pour the mixed solution into a suction filtration bottle, filter and wash it with deionized water until the pH value reaches 7, dry the obtained powder in a drying oven at 90°C, ball-mill the powder and sieve the powder to collect the powder with a particle size less than 300 mesh, place the powder in a muffle furnace and keep it at 300°C for 6 hours, then pass the powder into an argon-hydrogen mixed gas (40% hydrogen) at 950°C and keep it at this temperature for 3 hours, and the obtained powder is used as sintering powder.
[0070] (2) The powder is sintered in a spark plasma device at a heating rate of 50°C / min, a sintering pressure of 40 MPa, a sintering temperature of 1600°C, and a holding time of 10 min to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0071] Example 2
[0072] (1) Add carbon nanotubes to deionized water and disperse them by ultrasonic to obtain a carbon nanotube slurry with a mass fraction of 0.1%, then add phosphotungstic acid to the carbon nanotube slurry and stir it in a stirrer for four days. The mass ratio of phosphotungstic acid to carbon nanotubes is 10:1. Pour the mixed solution into a suction filtration bottle, filter and wash it with deionized water until the pH value reaches 7, dry the obtained powder in a drying oven at 50°C, ball-mill the powder and sieve the powder to collect the powder with a particle size less than 300 mesh, place the powder in a muffle furnace and keep it at 100°C for 6 hours, then pass the powder into an argon-hydrogen mixed gas (40% hydrogen) at 950°C and keep it at 1 hour, and the obtained powder is used as sintering powder.
[0073] (2) The powder is sintered in a spark plasma device at a heating rate of 10°C / min, a sintering pressure of 20 MPa, a sintering temperature of 1000°C, and a holding time of 5 min to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0074] Example 3
[0075] (1) Add carbon nanotubes to deionized water and disperse them ultrasonically to obtain a carbon nanotube slurry with a mass fraction of 0.5%, then add phosphotungstic acid to the carbon nanotube slurry and stir it in a stirrer for four days. The mass ratio of phosphotungstic acid to carbon nanotubes is 40:1. Pour the mixed solution into a suction filtration bottle, filter and wash it with deionized water until the pH value reaches 7, dry the obtained powder in a drying oven at 100°C, ball-mill the powder and sieve the powder to collect the powder with a particle size less than 300 mesh, place the powder in a muffle furnace and keep it at 500°C for 6 hours, then pass the powder into an argon-hydrogen mixed gas (40% hydrogen) at 950°C and keep it at this temperature for 5 hours, and the obtained powder is used as sintering powder.
[0076] (2) The powder is sintered in a spark plasma device at a heating rate of 100°C / min, a sintering pressure of 60 MPa, a sintering temperature of 1600°C, and a holding time of 60 min to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0077] Example 4
[0078] (1) Add carbon nanotubes to deionized water and disperse them ultrasonically to obtain a carbon nanotube slurry with a mass fraction of 0.2%, then add phosphotungstic acid to the carbon nanotube slurry and stir it in a mixer for four days. The mass ratio of phosphotungstic acid to carbon nanotubes is 25:1. Pour the mixed solution into a suction filtration bottle, filter and wash it with deionized water until the pH value reaches 7, dry the obtained powder in a drying oven at 100°C, ball-mill the powder and sieve the powder to collect the powder with a particle size less than 300 mesh, place the powder in a muffle furnace and keep it at 200°C for 10 hours, then pass the powder into an argon-hydrogen mixed gas (20% hydrogen) at 800°C and keep it at this temperature for 3 hours, and the obtained powder is used as sintering powder.
[0079] (2) The powder is sintered in a spark plasma device at a heating rate of 80°C / min, a sintering pressure of 50 MPa, a sintering temperature of 1500°C, and a holding time of 30 min to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0080] Example 5
[0081] (1) Add carbon nanotubes to deionized water and disperse them ultrasonically to obtain a carbon nanotube slurry with a mass fraction of 0.4%, then add phosphotungstic acid to the carbon nanotube slurry and stir it in a mixer for four days. The mass ratio of phosphotungstic acid to carbon nanotubes is 30:1. Pour the mixed solution into a suction filtration bottle, filter and wash it with deionized water until the pH value reaches 7, dry the obtained powder in a drying oven at 100°C, ball-mill the powder and sieve the powder to collect the powder with a particle size less than 300 mesh, place the powder in a muffle furnace and keep it at 300°C for 4 hours, then pass the powder into an argon-hydrogen mixed gas (30% hydrogen) at 600°C and keep it at this temperature for 5 hours, and the obtained powder is used as sintering powder.
[0082] (2) The powder was sintered in a spark plasma device at a heating rate of 30°C / min, a sintering pressure of 30 MPa, a sintering temperature of 1200°C, and a holding time of 40 min to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
[0083] For the transmission electron microscope image of the tungsten carbide embedded carbon nanotube powder obtained in step (1) of Example 1 of the present invention, please refer to Figure 2 As shown, from Figure 2 It can be seen that tungsten carbide nanowires achieve confined growth within carbon nanotubes, and the preparation of tungsten carbide embedded carbon nanotube powder is successfully realized.
[0084] Figure 3 and Figure 4 The actual image and cross-sectional scanning electron microscope image of the tungsten carbide embedded carbon nanotube bulk composite material sample obtained in step (2) of Example 1 respectively show that spark plasma sintering can effectively realize the assembly of tungsten carbide embedded carbon nanotubes, while the one-dimensional morphological characteristics of carbon nanotubes are still retained at the microscopic level.
[0085] X-ray diffraction analysis was performed on tungsten carbide embedded carbon nanotube powder, tungsten carbide embedded carbon nanotube bulk composite material and ablated surface, such as Figure 5 As shown, it can be clearly seen that the tungsten carbide embedded carbon nanotube powder mainly has the C peak, W2C peak and W peak of carbon nanotubes, and the tungsten carbide embedded carbon nanotube bulk composite material sample obtained by spark plasma sintering mainly has the C peak, W2C peak and WC peak of carbon nanotubes.
[0086] The load and penetration depth of the indenter were measured in real time on the surface of the polished sample using a nanoindenter (Nano Indenter G200, KLA), and the hardness and elastic modulus of the tungsten carbide embedded carbon nanotube bulk composite material were calculated based on the load-displacement curve. In this embodiment, an indenter was selected for testing, with a maximum load of 100 mN and a holding time of 30 s.
[0087] Figure 6 Table 1 shows the instrumented micrometer indentation load-displacement curves of carbon nanotubes and tungsten carbide embedded carbon nanotube bulk composites and their measured mechanical properties. Figure 6 The curve of the indentation depth changing with the sliding stroke is shown. The results show that the mechanical properties of carbon nanotubes are significantly improved after filling tungsten carbide nanowires. Compared with the carbon nanotube samples, the hardness and elastic modulus of the tungsten carbide embedded carbon nanotube bulk composite material samples increased by 22% and 43% respectively, indicating that filling tungsten carbide nanowires can significantly improve the mechanical properties of carbon nanotube bulk.
[0088] Table 1 Hardness and elastic modulus of carbon nanotubes and tungsten carbide embedded carbon nanotube bulk composites
[0089]
[0090]
[0091] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0092] It should be understood that the above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this field, other modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a bulk composite material of tungsten carbide embedded with carbon nanotubes, characterized in that: include: Mixing carbon nanotube slurry and phosphotungstic acid, filtering, and drying to obtain phosphotungstic acid embedded carbon nanotube powder; The phosphotungstic acid embedded carbon nanotube powder is subjected to reduction treatment, so that tungsten carbide nanowires are confined and filled in the carbon nanotubes to grow, thereby obtaining tungsten carbide embedded carbon nanotube powder; The tungsten carbide embedded carbon nanotube powder is subjected to spark plasma sintering to obtain a tungsten carbide embedded carbon nanotube bulk composite material.
2. The preparation method according to claim 1, characterized in that: include: The carbon nanotubes are ultrasonically dispersed in water to obtain carbon nanotube slurry; preferably, the mass fraction of the carbon nanotube slurry is 0.1-0.5%.
3. The preparation method according to claim 1, characterized in that: include: Adding phosphotungstic acid to the carbon nanotube slurry, stirring and mixing, filtering the obtained mixed solution, drying, ball milling, and sieving to obtain a mixed powder; Preferably, the mass ratio of the phosphotungstic acid to the carbon nanotubes is 10:1 to 40:1; Preferably, the stirring time is 1 to 6 days; Preferably, the particle size of the phosphotungstic acid embedded carbon nanotube powder is 100-300 meshes.
4. The preparation method according to claim 1, characterized in that: include: The phosphotungstic acid embedded carbon nanotube powder is heated at 100-500° C. for 4-10 hours, then heated to 600-950° C., and subjected to reduction treatment in a reducing atmosphere for 1-5 hours to obtain tungsten carbide embedded carbon nanotube powder; Preferably, the reducing atmosphere comprises a mixed atmosphere of hydrogen and an inert gas; particularly preferably, the volume percentage of hydrogen in the mixed atmosphere is 20 to 40%.
5. The preparation method according to claim 1, characterized in that: The content of phosphotungstic acid in the phosphotungstic acid embedded carbon nanotube powder is 20-50wt%; and / or the diameter of the tungsten carbide nanowire is 0.5-4nm.
6. The preparation method according to claim 1, characterized in that: include: Placing the tungsten carbide embedded carbon nanotube powder in a graphite mold, and then placing it in a spark plasma sintering system, compacting the tungsten carbide embedded carbon nanotube powder, and evacuating the spark plasma sintering system; The graphite mold is heated, and pressure is applied to both ends of the compacted tungsten carbide embedded carbon nanotube powder, thereby performing the spark plasma sintering.
7. The preparation method according to claim 6, characterized in that: include: The graphite mold is heated at a heating rate of 10-100°C / min to raise the temperature to 1000-1600°C, and the pressure applied to both ends of the compacted tungsten carbide embedded carbon nanotube powder is 20-60MPa; the spark plasma sintering time is 5-60min.
8. A bulk composite material of tungsten carbide embedded with carbon nanotubes prepared by the preparation method according to any one of claims 1 to 7.
9. The tungsten carbide embedded carbon nanotube bulk composite material according to claim 8, characterized in that: The tungsten carbide embedded carbon nanotube bulk composite material has a hardness of 540-1000 MPa and an elastic modulus of 4-10 GPa.
10. Application of the tungsten carbide embedded carbon nanotube bulk composite material according to claim 8 or 9 in the field of aerospace.
Citation Information
Patent Citations
CNTs toughening WC composite material and preparing method thereof
CN105503230A
Preparation method of NiCo2O4@carbon nanotube composite material
CN106328393A
Preparation process of diamond and carbon nanotube composite cutting pick
CN116160005A
Method for preparing superfine nanoparticle / line-at-single-wall carbon nanotube composite macroscopic body
CN118359188A
Rod-shaped ceramic resistant heating body useful for guide- and calendar rollers in polymer film technique, comprises carbon nanotubes embedded as electric conductive phase in a silicate- or oxide ceramic matrix