Method for improving brazing binding force of aluminum nitride heater assembly

By improving the cooked ceramic, tungsten is wetted into the inside of the ceramic and soldered with active solder, the problem of insufficient brazing bonding force of the aluminum nitride heater assembly is solved, and the binding strength is significantly improved.

CN118930302APending Publication Date: 2024-11-12合肥商德应用材料有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411050161.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The brazing bonding force of existing aluminum nitride heater components is difficult to meet the high bonding force requirements.

Method used

By improving the cooked ceramic, the tungsten slurry is applied and passed through the glue discharge and sintering and smooth grinding process to make the tungsten wet into the inside of the ceramic, and then soldering is performed using active solder such as silver copper titanium solder.

Benefits of technology

The brazing bonding force of the aluminum nitride heater assembly is significantly improved to meet the demand for high bonding force.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930302A_ABST
    Figure CN118930302A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the brazing binding force of an aluminum nitride heater assembly, and relates to the technical field of aluminum nitride heater assembly production, and the method comprises the following steps: S1, carrying out improvement treatment on a cooked blank ceramic, so that tungsten is infiltrated into the ceramic; s2, a metal electrode and a temperature sensor are placed at the welding position of the cooked blank ceramic; and S3, through filling of the active welding flux, the cooked body ceramic is welded to a metal electrode and a temperature sensor, and the aluminum nitride heater assembly is obtained.The improved cooked body ceramic is obtained through the procedures of improving the cooked body ceramic, smearing the surface of the green body with the tungsten slurry and conducting glue discharging, sintering and flat grinding, and the aluminum nitride heater assembly is obtained. At the moment, after the tungsten slurry and the ceramic are co-fired in the brazing area of the cooked blank ceramic, tungsten in the brazing area is thoroughly and uniformly soaked, then brazing with other parts is carried out by filling active welding flux, the binding force strength after brazing is obviously improved, and the use requirement of the aluminum nitride heater assembly in a high-binding-force requirement scene is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum nitride heater assembly production, and in particular to a method for improving the brazing bonding strength of an aluminum nitride heater assembly. Background Art

[0002] The aluminum nitride heater assembly is composed of three parts: a preformed ceramic (with a circuit), a metal electrode and a temperature sensor. The aluminum nitride heater assembly is obtained by brazing the preformed ceramic (with a circuit), the metal electrode and the temperature sensor.

[0003] The welding strength between the raw ceramic and other components is one of the key indicators of the brazing quality of aluminum nitride heater components. At present, the brazing process often uses silver-copper-titanium solder. The titanium in silver-copper-titanium has good wettability for aluminum nitride ceramics, which increases the welding strength to a certain extent. However, for products with high bonding requirements, the existing brazing methods are still difficult to meet the requirements of brazing bonding strength. Therefore, a method for improving the brazing bonding strength of aluminum nitride heater components is needed to solve the above problems. Summary of the invention

[0004] The object of the present invention is to provide a method for improving the brazing bonding strength of an aluminum nitride heater assembly, so as to solve the problems existing in the prior art mentioned in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for improving the brazing bonding strength of an aluminum nitride heater assembly comprises the following steps:

[0007] S1: Improve the cooked ceramic so that tungsten can be infiltrated into the ceramic;

[0008] S2: placing the metal electrode and the temperature sensor at the welding position of the cooked ceramic;

[0009] S3: By filling active solder, the cooked ceramic is welded with the metal electrode and the temperature sensor to obtain an aluminum nitride heater assembly.

[0010] Preferably, the specific steps of improving the cooked ceramic in S1 are:

[0011] In the process of making cooked ceramics, the green body is improved by applying tungsten slurry to the surface of the green body after the green body fine carving process, and then going through the processes of debinding sintering and flat grinding to obtain the improved cooked ceramics.

[0012] Preferably, the tungsten slurry comprises a tungsten powder mixture and a solvent, wherein the tungsten powder mixture comprises 0-5% by weight of aluminum nitride powder and the rest is tungsten powder.

[0013] Preferably, the area where the tungsten slurry is applied is a pre-brazing area in a green state.

[0014] Preferably, the active solder in S3 is silver-copper-titanium solder.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] The present invention improves the cooked ceramic, applies tungsten slurry to the surface of the green ceramic, and then carries out the debinding sintering and flat grinding processes to obtain the improved cooked ceramic. At this time, after the brazing area of ​​the cooked ceramic is co-fired with the tungsten slurry and the ceramic, the tungsten infiltrates into the interior of the ceramic, so that the tungsten in the brazing area is deeply and evenly infiltrated. Then, by filling active solder to braze with other components, the bonding strength is significantly increased after brazing, which meets the use requirements of the aluminum nitride heater assembly in scenarios with high bonding strength requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a photograph of a green body coated with tungsten slurry according to the present invention.

[0018] Figure 2 This is a photograph of a processed blank coated with tungsten slurry according to the present invention.

[0019] Figure 3 This is a photo of the aluminum nitride heater assembly that has been welded according to the present invention. DETAILED DESCRIPTION

[0020] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0021] See also Figure 1-3 , the present invention provides the following technical solutions:

[0022] A method for improving the brazing bonding strength of an aluminum nitride heater assembly comprises the following steps:

[0023] S1: Improve the cooked ceramics so that tungsten can penetrate into the interior of the ceramics; cooked ceramics (with circuits) are mainly made by casting, printing, laminating, green body carving, binder removal sintering, and flat grinding. The specific steps of improving the cooked ceramics are: in the process of making cooked ceramics, the green body after the green body carving process is improved, that is, tungsten slurry is applied to the surface of the green body, and then the binder removal sintering and flat grinding process are carried out to obtain the improved cooked ceramics.

[0024] The area where the tungsten slurry is applied is the pre-brazing area in the green state, and only the pre-brazing area needs to be applied, which can save the use of tungsten slurry and reduce production costs.

[0025] The tungsten slurry comprises a tungsten powder mixture and a solvent, wherein the solvent mainly contains diethylene glycol monobutyl ether and pinene alcohol. The tungsten powder mixture comprises 0-5% by weight of aluminum nitride powder, and the rest is tungsten powder.

[0026] S2: placing the metal electrode and the temperature sensor at the welding position of the raw ceramic.

[0027] S3: The cooked ceramic is welded with the metal electrode and the temperature sensor by filling with active solder to obtain an aluminum nitride heater assembly; the active solder in S3 is silver-copper-titanium solder, and the titanium in the silver-copper-titanium solder has good wettability for aluminum nitride ceramics, and can be combined with the improved cooked ceramic to further improve the welding strength. At the same time, other active solders can also be used for welding.

[0028] Take 3 samples A and 3 samples B, sample A is an aluminum nitride heater component that has not been improved on the cooked ceramic, and sample B is an aluminum nitride heater component that has been improved on the cooked ceramic. Other production processes and parameters are the same, and silver-copper-titanium solder is used for welding. After brazing, the 6 aluminum nitride heater components are subjected to tensile tests, and the test results are shown in the following table:

[0029] Group 1 Group 2 Group 3 Sample A 32kg 31kg 32kg Sample B 46kg 48kg 47kg

[0030] It can be concluded from the above test results that the pull-out force of the aluminum nitride heater component sample after the improved treatment of the cooked ceramic is significantly greater than that of the aluminum nitride heater component without the improved treatment of the cooked ceramic.

[0031] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for improving the brazing bonding strength of an aluminum nitride heater assembly, characterized in that: The steps include: S1: Improve the cooked ceramic so that tungsten can be infiltrated into the ceramic; S2: placing the metal electrode and the temperature sensor at the welding position of the cooked ceramic; S3: By filling active solder, the cooked ceramic is welded with the metal electrode and the temperature sensor to obtain an aluminum nitride heater assembly.

2. A method for improving the brazing bonding strength of an aluminum nitride heater assembly according to claim 1, characterized in that: The specific steps of the improved treatment of the sintered ceramic in S1 are: In the process of making cooked ceramics, the green body is improved by applying tungsten slurry to the surface of the green body after the green body fine carving process, and then going through the processes of debinding sintering and flat grinding to obtain the improved cooked ceramics.

3. A method for improving the brazing bonding strength of an aluminum nitride heater assembly according to claim 2, characterized in that: The tungsten slurry comprises a tungsten powder mixture and a solvent. The tungsten powder mixture comprises 0-5% by weight of aluminum nitride powder and the rest is tungsten powder.

4. A method for improving the brazing bonding strength of an aluminum nitride heater assembly according to claim 2, characterized in that: The area where the tungsten slurry is applied is a pre-brazing area in a green state.

5. The method for improving the brazing bonding strength of an aluminum nitride heater assembly according to claim 1, characterized in that: The active solder in S3 is silver-copper-titanium solder.

Citation Information

Patent Citations

  • Manufacturing method for ceramic heating element

    CN108882405A

  • High-temperature co-fired ceramic metallization slurry and preparation method thereof

    CN118084541A

  • Brazing filler metal

    JP2000158180A