Method for preparing silicon fertilizer from quartz vein type gold ore tailings

The quartz vein-type gold mine tailings are treated by mechanochemical method, which converts harmful elements into stable sulfides and increases the effective silicon content of silicon fertilizers, solving the impact of harmful elements in tailings on plants and the inability to absorb silicon elements, realizing the problem of the impact of harmful elements in tailings. The preparation of high-value-added nano-silicon fertilizers has been improved, and the yield and production simplicity are improved.

CN118930333APending Publication Date: 2024-11-12THE SIXTH GEOLOGICAL TEAM OF SHAANXI GEOLOGY & MINERAL RESOURCES CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411167863.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Quartz vein-type gold tailings contain elements that are harmful to plants such as Al, Pb, Pt, Cd and Hg, which affects plant growth, and silicon elements cannot be absorbed by plants, resulting in low added value of fertilizers and cannot be effectively treated by conventional flotation processes. Micro-grained minerals.

Method used

After grinding the quartz vein gold tailings in a ball mill by one-step mechanochemistry, water and HCl are added to adjust the pH value, and flotation is performed using sodium dodecyl sulfate and thiolated modified cellulose supported by metal oxides. , convert harmful metal elements into stable sulfides, increase the hydrophobicity of aluminum, and obtain high-value nano-silicon fertilizer through high-speed ball milling.

Benefits of technology

It effectively reduces the potential harm of heavy metals to soil and plants, increases the effective silicon content of nano-silicon fertilizers and the content of aluminum and other heavy metal ions, increases crop yields, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930333A_ABST
    Figure CN118930333A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a silicon fertilizer from quartz vein type gold ore tailings. The method comprises the steps that firstly, the quartz vein type gold ore tailings are placed in a ball mill to be ground for 15-20 h at the speed of 400-500 rpm till 70%-80% of the tailings with the particle size smaller than 20 micrometers are obtained, water is added for mixing, ore pulp with the concentration being 20%-40% is obtained and poured into a flotation tank, HCl with the concentration being 0.2 mol / L is added, the PH value is adjusted to be 3.5-4.5, and the flotation tank is used for flotation; then an inhibitor, a lauryl sodium sulfate aqueous solution with the concentration being 5%-8% and a foaming agent are added according to the amount of 100-200 g / t ore, 200-500 g / t ore and 20-40 g / t ore respectively, ore pulp is adjusted for 2-3 min at the speed of 400-600 rpm, and flotation time is 5-7 min; after concentrate obtained through flotation is dried, sulfhydrylation modified cellulose loaded with metal oxide is added according to the amount of 10-20 kg / t ore, high-speed ball milling is conducted for 3-5 h, and the nano silicon fertilizer with the high additional value is obtained. By adopting the method, the quartz vein type gold ore tailings can be converted into the nano silicon fertilizer, the content of effective silicon is high, the content of aluminum and other heavy metal ions is extremely low, the crop yield can be increased, and in addition, the method is simple, easy to operate and suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a method for preparing silicon fertilizer by utilizing quartz vein type gold mine tailings. Background Art

[0002] Quartz vein gold mine tailings refer to the waste generated during the mining process of quartz veins in gold mines. Since most of the gold ore is composed of quartz, feldspar and other substances, a large amount of tailings are produced during the gold flotation process. These tailings are usually piled up in tailings ponds near the mining area, which not only occupies land resources, but also may cause environmental pollution. Therefore, it is of great significance to effectively utilize gold mine tailings.

[0003] The main component of gold tailings is quartz sand, and it also contains a small amount of Ca, Ba, B, Co, Ga, Mn, Nb and other elements that are beneficial to plants. These elements can be added to silicon fertilizer to increase the added value of silicon fertilizer. However, there are two problems in using gold tailings to prepare silicon fertilizer: first, the tailings contain a small amount of elements that are harmful to plants, such as Al, Pb, Pt, Cd and Hg; the aluminum ions in the quartz vein gold tailings will affect the permeability of the root cell membrane, interfere with the plant's absorption of water, and thus affect the root growth. High concentrations of aluminum may cause the death of root tip cells, reduce root branching, and affect the plant's water absorption capacity and nutrient absorption. Lead ions will affect the development of plant roots, and will also interfere with the plant's absorption and utilization of essential nutrients, such as nitrogen, phosphorus, potassium, etc., leading to nutritional imbalance, thereby interfering with the growth and development process of plants, causing slow plant growth, and ultimately affecting the yield and quality of plants. Due to the complex intercalation relationship between lead minerals and gangue minerals, the recovery of fine lead minerals is difficult. Conventional flotation processes cannot effectively process these fine minerals. Another problem is that the silicon in gold tailings cannot be absorbed by plants due to its existence form and cannot be directly used as fertilizer.

[0004] In view of the above problems, the present invention aims to provide a method for preparing silicon fertilizer using quartz vein-type gold mine tailings by a one-step mechanochemical method. Summary of the invention

[0005] The purpose of the invention is to provide a method for preparing silicon fertilizer by utilizing quartz vein type gold mine tailings.

[0006] The object of the present invention is achieved in this way. A method for preparing silicon fertilizer using quartz vein type gold mine tailings is achieved by the following steps: 1) First, place the quartz vein gold tailings in a ball mill at a speed of 400-500rpm for 15-20h until the particle size is less than 20 microns, accounting for 70-80%. Add water to mix to obtain a slurry with a concentration of 20-40%. Pour it into the flotation tank, add 0.2mol / L HCl to adjust the pH value to 3.5-4.5, and then adjust the pH value according to 100-200 g / t 矿 , 200-500g / t 矿 , 20-40g / t 矿 Add inhibitor, 5%-8% sodium dodecyl sulfate aqueous solution and frother respectively, adjust the pulp at 400-600rpm for 2-3min, and the flotation time is 5-7min; 2) After the concentrate obtained by flotation is dried, the concentration is 10-20kg / t 矿 The amount of thiolated modified cellulose loaded with metal oxides was added and the mixture was ball-milled at high speed for 3-5 hours to obtain high value-added nano-silicon fertilizer.

[0007] In the flotation process of the present invention, sodium dodecyl sulfate is used to react or adsorb on the surface of aluminum minerals to increase the surface hydrophobicity of aluminum minerals, thereby promoting their flotation and realizing the separation of aluminum. The present invention adds a certain amount of thiol-modified cellulose loaded with metal oxides to the gold tailings, and converts Pb, Pt, Cd, and Hg into sulfides by a mechanochemical method. The sulfides of these harmful metal elements are very stable, and will not be hydrolyzed to release metal ions even under acidic conditions, and will not be absorbed by plants. Converting these heavy metals into sulfides can reduce their migration, toxicity, and the risk of plant absorption in the soil, which helps to reduce the potential harm of heavy metals to soil organisms and ecosystems. At the same time, in this process, part of the silicon dioxide is converted into silicates with good water solubility, which are easily absorbed by plants.

[0008] The beneficial effects of the present invention are as follows: the method of the present invention can transform quartz vein-type gold mine tailings into nano silicon fertilizers, which have high effective silicon content and extremely low aluminum and other heavy metal ion contents, and can improve crop yields. In addition, the method of the present invention is simple and easy to operate, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 This is an electron microscope image of the nano-silicon fertilizer prepared in Example 1. DETAILED DESCRIPTION

[0010] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.

[0011] The present invention provides a method for preparing silicon fertilizer by using quartz vein type gold mine tailings, which is achieved by the following steps: 1) First, place the quartz vein gold tailings in a ball mill at a speed of 400-500rpm for 15-20h until the particle size is less than 20 microns, accounting for 70-80%. Add water to mix to obtain a slurry with a concentration of 20-40%. Pour it into the flotation tank, add 0.2mol / L HCl to adjust the pH value to 3.5-4.5, and then adjust the pH value according to 100-200 g / t 矿 , 200-500g / t 矿 , 20-40g / t 矿 Add inhibitor, 5%-8% sodium dodecyl sulfate aqueous solution and frother respectively, adjust the pulp at 400-600rpm for 2-3min, and the flotation time is 5-7min; 2) After the concentrate obtained by flotation is dried, it is sold at 10-20kg / t 矿 The amount of thiolated modified cellulose loaded with metal oxides was added and the mixture was ball-milled at high speed for 3-5 hours to obtain high value-added nano-silicon fertilizer.

[0012] The preparation method of the thiol-modified cellulose loaded with metal oxide is as follows: After the thioglycolic acid-modified cellulose is soaked with ethanol, 50-70 ml of a suspension of magnesium oxide or calcium oxide powder is slowly added dropwise while stirring. After continuous stirring for 1-2 hours, the mixture is filtered and the filter residue is dried at 80-100 °C. The stirring speed is 250-350 rpm.

[0013] The mass ratio of thioglycolic acid-modified cellulose to magnesium oxide or calcium oxide powder is 10:4-6, and each ml of the suspension contains 80-90 mg of magnesium oxide or calcium oxide powder.

[0014] The mass volume ratio of thioglycolic acid-modified cellulose to ethanol is 1:10-14 g / ml.

[0015] The preparation method of the thioglycolic acid-modified cellulose is as follows: cellulose is added to thioglycolic acid with a concentration of 20-30 g / L, mixed evenly, and stirred at a speed of 200-220 rpm for reaction for 2-3 h at room temperature to obtain thioglycolic acid-modified cellulose, wherein the mass volume ratio of cellulose to thioglycolic acid is 1:20-24 g / ml.

[0016] In step 1), the inhibitor is sodium hexametaphosphate, and the foaming agent is No. 2 oil.

[0017] In step 2), the high-speed ball milling speed is 1000-1200 rpm.

[0018] The contents of Al, Pb, Pt, Cd and Hg in the quartz vein gold mine tailings treated in the following examples are 1.76%, 0.002%, 0.03%, 0.004% and 0.0006%, respectively.

[0019] Example 1 First, put the quartz vein-type gold mine tailings into a ball mill for grinding at a speed of 400rpm and a grinding time of 15h, so that the particle size of the ore sample is less than 20 microns. Mix 100g of the ground tailings with 400ml of water and pour it into a flotation tank to obtain a slurry with a mass concentration of 20%. Add 0.2mol / L HCl to adjust the pH value to 3.5, and then add 0.01g of sodium hexametaphosphate as an inhibitor. Add 0.02g of a 5% aqueous solution of sodium dodecyl sulfate as a collector. Add 0.002g of No. 2 oil and adjust the slurry time to 2min. Adjust the slurry stirring speed to 400rpm for 5min; 10 g of the concentrate sample after flotation was mixed with 0.04 g of thiolated modified cellulose loaded with metal oxides and subjected to high-speed ball milling, with the ball milling speed set at 1000 rpm and the ball milling time set at 3 h. High value-added nano-silicon fertilizer was obtained by ball milling.

[0020] The preparation method of the thiolated modified cellulose loaded with metal oxide is as follows: 1. Add 10 g of cellulose to 200 ml of 20 g / L thioglycolic acid, mix well, react at room temperature for 2 h and stir at 200 rpm. Through chemical reaction, the thiol group is grafted onto the molecular chain of cellulose to obtain thioglycolic acid-modified cellulose.

[0021] 2. Place 10 g of modified cellulose material in a beaker and soak it with 100 ml of ethanol to enhance the subsequent loading effect of metal oxides. Accurately weigh 4 g of magnesium oxide powder, set the stirring speed to 250 rpm, and evenly disperse it in 50 ml of deionized water to form a suspension.

[0022] 3. Slowly add the above suspension to the impregnated cellulose material and stir it at 200 rpm for 1 h to ensure that the metal oxide is evenly loaded on the cellulose surface. After loading, filter the mixture and dry it at 80 °C to remove excess solvent.

[0023] Example 2 First, the quartz vein-type gold mine tailings were ground in a ball mill at a speed of 400 rpm for 15 h, so that the particle size of the ore sample was less than 20 microns. 100 g of the ground ore was mixed with 300 ml of water and poured into a flotation cell to obtain a slurry with a mass concentration of 25%. 0.2 mol / L HCl was added to adjust the pH value to 4, and then 0.015 g of sodium hexametaphosphate was added as an inhibitor. 0.035 g of a 6% aqueous solution of sodium dodecyl sulfate was added as a collector. 0.003 g of No. 2 oil was added and the slurry time was adjusted to 3 min. The slurry stirring speed was adjusted to 500 rpm and the flotation time was 6 min. 10 g of the concentrate sample after flotation was mixed with 0.15 g of thiolated modified cellulose loaded with metal oxides and subjected to high-speed ball milling. The ball milling speed was set to 1100 rpm and the ball milling time was 4 h. High value-added nano-silicon fertilizer was obtained by ball milling.

[0024] The preparation method of the thiol-modified cellulose loaded with metal oxide is as follows: 1. Add 10 g of cellulose to 220 ml of 25 g / L thioglycolic acid, mix well, react at room temperature for 2.5 h and stir at 210 rpm. Through chemical reaction, the thiol group is grafted onto the molecular chain of cellulose to obtain thioglycolic acid-modified cellulose.

[0025] 2. Place 10 g of modified cellulose material in a beaker and soak it with 110 ml of ethanol to enhance the subsequent loading effect of metal oxides. Accurately weigh 5 g of calcium oxide powder, set the stirring speed to 300 rpm, and evenly disperse it in 60 ml of deionized water to form a suspension.

[0026] 3. Slowly add the above suspension to the impregnated cellulose material and stir it at 300 rpm for 1.5 h to ensure that the metal oxide is evenly loaded on the cellulose surface. After loading, filter the mixture and dry it at 90 °C to remove excess solvent.

[0027] Example 3 First, put the quartz vein gold tailings into a ball mill for grinding at a speed of 400 rpm and a grinding time of 15 h, so that the particle size of the ore sample is less than 20 microns. Mix 100 g of the ground ore with 150 ml of water and pour it into the flotation tank to obtain a slurry with a mass concentration of 40%. Add 0.2 mol / L HCl to adjust the pH value to 4.5, and then add 0.02 g of sodium hexametaphosphate as an inhibitor. Add 0.05 g of 8% sodium dodecyl sulfate aqueous solution as a collector. Add 0.004 g of No. 2 oil and adjust the slurry time to 3 min. Adjust the slurry stirring speed to 600 rpm and the flotation time to 7 min; 10 g of the concentrate sample after flotation was mixed with 0.2 g of thiolated modified cellulose loaded with metal oxides and subjected to high-speed ball milling. The ball milling speed was set to 1200 rpm and the ball milling time was 5 h. High value-added nano-silicon fertilizer was obtained by ball milling.

[0028] The preparation method of the thiolated modified cellulose loaded with metal oxide is as follows: 1. Add 10 g of cellulose to 240 ml of 30 g / L thioglycolic acid, mix well, react at room temperature for 3 h and stir at 220 rpm. Through chemical reaction, the thiol group is grafted onto the molecular chain of cellulose to obtain thioglycolic acid-modified cellulose.

[0029] 2. Place 10 g of modified cellulose material in a beaker and soak it with 140 ml of ethanol to enhance the subsequent loading effect of metal oxides. Accurately weigh 6 g of magnesium oxide or calcium oxide powder, set the stirring speed to 350 rpm, and evenly disperse it in 70 ml of deionized water to form a suspension.

[0030] 3. Slowly add the above suspension to the impregnated cellulose material and stir it at 400 rpm for 2 h to ensure that the metal oxide is evenly loaded on the cellulose surface. After loading, filter the mixture and dry it at 100 °C to remove excess solvent.

[0031] Comparative Example 1 The difference between this comparative example and Example 1 is that the concentrate obtained by flotation is used as silicon fertilizer.

[0032] Comparative Example 2 The difference between this comparative example and Example 1 is that the cellulose without any modification and the concentrate sample after flotation are subjected to high-speed ball milling to obtain silicon fertilizer.

[0033] Comparative Example 3 The difference between this comparative example and Example 1 is that the thioglycolic acid-modified cellulose and the concentrate sample after flotation are subjected to high-speed ball milling to obtain silicon fertilizer.

[0034] Comparative Example 4 The difference between this comparative example and Example 1 is that the cellulose loaded with only metal oxides and the concentrate sample after flotation are subjected to high-speed ball milling to obtain silicon fertilizer.

[0035] The preparation method of cellulose loaded with metal oxides is as follows: 10 g of cellulose material is placed in a beaker and soaked with 100 ml of ethanol to enhance the subsequent loading effect of metal oxides. Accurately weigh 4 g of magnesium oxide powder, set the stirring speed to 250 rpm, and evenly disperse it in deionized water to form a suspension. Slowly add the above suspension to the soaked cellulose material, and continue stirring at a speed of 200-400 rpm to ensure that the metal oxide is evenly loaded on the cellulose surface. After the loading is completed, the mixture is filtered and dried at 80 °C to remove excess solvent.

[0036] Comparative Example 5 This comparative example is selected from commercially available silicon fertilizer.

[0037] Experimental Example 1 Detection of Particle Size and Equivalent SiO2 Content of Silicon Fertilizers in Examples 1-3 and Comparative Examples 1-5 and Detection of Ion Conversion Rates of Al, Pb, Pt, Cd, and Hg The results are shown in Table 1.

[0038] Table 1 Particle size and composition of silicon fertilizers in Examples 1-3 and Comparative Examples 1-5 As can be seen from Table 1, the silicon fertilizers prepared in Examples 1-3 have a higher effective silicon content and are more conducive to plant growth. In addition, the silicon fertilizer preparation method used in Examples 1-3 can achieve a higher conversion rate of heavy metal element ions such as Pb, Pt, Cd, and Hg, reducing the impact on soil and plant growth.

[0039] Experimental Example 2 Detection of the effect of silicon fertilizer on the physical indexes of rice in Example 1-3 1. Experimental methods: 1. The experimental area is 20 m² (5 m long and 4 m wide), and ridges are set up to isolate the intervals to prevent fertilizer and water from flowing.

[0040] 2. Fertilization plan: Before transplanting rice, mix silicon fertilizer and base fertilizer evenly and apply them into the soil. The application rate of silicon fertilizer is 20g / m 2 The base fertilizer usage is 40g / m 2 . At the tillering stage and booting stage of rice, apply 10 g / m 2 Silicon fertilizer: Use spraying method to apply fertilizer, dilute it 1000 times with water, and spray it on the leaves.

[0041] 3. Measurement methods of rice physical indicators Plant height: During the rice maturity period, 10 rice plants were randomly selected from each area, and the height from the ground to the top of the ear was measured, and the average value was taken.

[0042] Ear length: The length of each ear was measured, and 10 ears were randomly selected from each area and the average value was taken.

[0043] Thousand-grain weight: 1000 grains were randomly selected from the harvested rice in each plot, weighed, repeated 3 times, and the average value was taken.

[0044] 2. Results: The effects of the silicon fertilizers obtained in Examples 1-3 of the present invention and Comparative Examples 1-5 on the physical indicators of rice are shown in Table 2.

[0045] Table 2 Effects of silicon fertilizers obtained in Examples 1-3 and Comparative Example 1 on the physical indicators of rice It can be seen from Table 2 that the silicon fertilizers prepared in Examples 1-3 of the present invention are more conducive to the growth of rice than those prepared in Comparative Examples 1-5.

Claims

1. A method for preparing silicon fertilizer using quartz vein type gold mine tailings, characterized in that: To do this, follow these steps: 1) First, place the quartz vein gold tailings in a ball mill at a speed of 400-500rpm and grind for 15-20h until the particle size is less than 20 microns, accounting for 70-80%. Add water to mix to obtain a slurry with a concentration of 20-40%. Pour it into the flotation tank, add 0.2mol / L HCl to adjust the pH value to 3.5-4.5, and then adjust it according to 100-200g / t 矿 , 200-500g / t 矿 , 20-40g / t 矿 Add inhibitor, 5%-8% sodium dodecyl sulfate aqueous solution and frother respectively, adjust the pulp at 400-600rpm for 2-3min, and the flotation time is 5-7min; 2) After the concentrate obtained by flotation is dried, it is sold at 10-20kg / t 矿 The amount of thiolated modified cellulose loaded with metal oxides was added and the mixture was ball-milled at high speed for 3-5 hours to obtain high value-added nano-silicon fertilizer.

2. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 1, characterized in that: The preparation method of the thiol-modified cellulose loaded with metal oxide is as follows: After the thioglycolic acid-modified cellulose is soaked with ethanol, 50-70 ml of a suspension of magnesium oxide or calcium oxide powder is slowly added dropwise while stirring, and the mixture is continuously stirred for 1-2 h and then filtered. The filter residue is dried at 80-100 °C to obtain the obtained product; The mass ratio of thioglycolic acid-modified cellulose to magnesium oxide or calcium oxide powder is 10:4-6, and each ml of the suspension contains 80-90 mg of magnesium oxide or calcium oxide powder.

3. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 2, characterized in that: The mass volume ratio of thioglycolic acid-modified cellulose to ethanol is 1:10-14 g / ml.

4. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 2, characterized in that: The stirring speed is 250-350 rpm.

5. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 2, characterized in that: The preparation method of the thioglycolic acid-modified cellulose is as follows: cellulose is added to thioglycolic acid with a concentration of 20-30 g / L, mixed evenly, and stirred at a speed of 200-220 rpm for reaction for 2-3 h at room temperature to obtain thioglycolic acid-modified cellulose, wherein the mass volume ratio of cellulose to thioglycolic acid is 1:20-24 g / ml.

6. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 1, characterized in that: In step 1), the inhibitor is sodium hexametaphosphate, and the foaming agent is No. 2 oil.

7. The method for preparing silicon fertilizer using quartz vein type gold mine tailings according to claim 1, characterized in that: In step 2), the high-speed ball milling speed is 1000-1200 rpm.