Waterproof real stone paint emulsion composition and preparation method thereof

By using monomers such as butyl acrylate and initiators in real stone paint emulsion, the problem of insufficient water resistance of real stone paint emulsion is solved, and better waterproof performance and stability are achieved. It is suitable for exterior wall coating of high-rise buildings. .

CN118930717APending Publication Date: 2024-11-12FOSHAN ROSF TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975256.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing real stone paint lotion is insufficient in outdoor applications, making it difficult to meet the waterproof performance needs of high-rise buildings.

Method used

Using butyl acrylate, functional monomer, mixed monomer, crosslinked monomer, silicone monomer, initiator and deionized water, a waterproof real stone paint emulsion is formed through specific formula ratios and preparation methods to enhance the The coating has low temperature resistance and waterproof properties.

Benefits of technology

It significantly improves the water resistance and waterproof performance of the coating, reduces the water absorption and whitening phenomenon of the coating, and improves the stability and uniformity of the emulsion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954339340000081
    Figure BDA0004954339340000081
Patent Text Reader

Abstract

The invention discloses a waterproof real stone paint emulsion composition and a preparation method thereof, and belongs to the technical field of paints.The waterproof real stone paint emulsion composition comprises butyl acrylate, a functional monomer, a mixed monomer, an acrylic monomer, a crosslinking monomer, an organosilicon monomer, an initiator, an emulsifier and deionized water; the butyl acrylate and the acrylic monomer in the formula system can enhance the low temperature resistance of the emulsion after film formation, and the soft characteristic of the emulsion helps the emulsion to form a better film, so that the waterproof performance is improved; by adding the organic silicon monomer, the waterproof performance of the coating can be improved, and the phenomenon that the coating absorbs water and becomes white is reduced; according to the present invention, the cross-linking monomer and other monomers are subjected to the cross-linking reaction to form the three-dimensional network structure so as to improve the water resistance of the coating, and the synergistic effect of various monomers and additives in the waterproof type real stone paint emulsion formula system, and the stability and the uniformity of the emulsion system are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, and in particular to a waterproof stone-like paint emulsion composition and its preparation method. Background Technology

[0002] Stone-like paint is a type of coating that closely resembles the decorative effect of marble and granite. It is primarily made by physically mixing high-performance polymer emulsions with various natural colored sands, stone powders, and functional additives. It possesses a natural and realistic color, giving a sense of elegance, harmony, and solemnity. Therefore, it visually and functionally replicates the effect of marble and granite. Furthermore, stone-like paint is lightweight, easy to apply, and inexpensive. It can be used on high-rise buildings, avoiding the dangers of marble or ceramic tiles falling from heights. As a result, stone-like paint is highly favored by builders and the market, leading to its rapid development in my country and making it one of the dominant coating materials in building exterior wall coating systems.

[0003] As the film-forming substance of stone paint, the emulsion plays a decisive role in the coating performance. Since stone paint is mainly used on outdoor exterior walls, it has extremely high requirements for the water resistance of the emulsion. Summary of the Invention

[0004] To address the aforementioned problems, this invention provides a waterproof stone-like paint emulsion composition and its preparation method. This waterproof stone-like paint emulsion exhibits excellent water resistance and weather resistance. The details of this invention are as follows:

[0005] The purpose of this invention is to provide a waterproof stone paint emulsion composition, the technical point of which is that, by weight parts, it comprises 71.5-89.5 parts of butyl acrylate, 20-30 parts of functional monomers, 0.2-0.3 parts of mixed monomers, 0.3-0.5 parts of acrylic monomers, 0.2-0.4 parts of crosslinking monomers, 0.3-0.5 parts of organosilicon monomers, 0.5-0.6 parts of initiator, 0.7-1.1 parts of emulsifier, and 70-100 parts of deionized water.

[0006] To better achieve the above technical solution, the functional monomer in the waterproof stone paint emulsion composition of the present invention is at least one of acrylamide, methyl acrylate monomer and N,N-methylenebisvinylamide.

[0007] To better achieve the above technical solution, the mixed monomer components and their mass percentages in the waterproof stone paint emulsion composition of the present invention are: 35-55% aromatic unsaturated monomers, 10-30% acrylate unsaturated monomers and 25-40% carboxyl-containing unsaturated monomers.

[0008] To better achieve the above technical solution, the acrylic acid in the waterproof stone paint emulsion composition of the present invention is at least one of acrylic acid and methacrylic acid.

[0009] To better achieve the above technical solution, the crosslinking monomer in the waterproof stone paint emulsion composition of the present invention is a mixture of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate, wherein the mass ratio of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate is (1-5):1.

[0010] To better achieve the above technical solution, the organosilicon monomer in the waterproof stone paint emulsion composition of the present invention is at least one of γ-methacryloyloxypropyltrimethylsilane and polydimethylsiloxane methacrylate.

[0011] To better achieve the above technical solution, the initiator in the waterproof stone paint emulsion composition of the present invention is at least one of potassium persulfate, ammonium persulfate and sodium persulfate.

[0012] To better achieve the above technical solution, the emulsifier in the waterproof stone paint emulsion composition of the present invention is at least one of polyoxyethylene sorbitan fatty acid ester and fatty alcohol polyoxyethylene ether.

[0013] Another objective of this invention is to provide a method for preparing a waterproof stone-like paint emulsion, the technical point of which includes the following steps:

[0014] Step 1: Add emulsifier and deionized water to the emulsification tank and stir at high speed. After the emulsifier is completely dissolved, add crosslinking monomer and pre-emulsify at high speed for 10-30 minutes to obtain pre-emulsion. Take out 5% as seed pre-emulsion for later use.

[0015] Step 2: Add butyl acrylate, functional monomers, mixed monomers, and acrylic monomers to the reactor and heat the mixture. When the temperature reaches 82-85℃, add the seed pre-emulsion from Step 1. After 1-3 minutes, add the initiator and continue to add the pre-emulsion from Step 1 dropwise for 1-2 hours. When the remaining amount of the pre-emulsion from Step 1 is 15-25%, add the organosilicon monomer mixture to the reactor and add it dropwise for 1-2 hours. After the addition is completed, keep the temperature for 1 hour, cool down to 70-80℃, keep the temperature for 20-40 minutes, and then cool down. Adjust the pH of the emulsion to 8.0 to obtain the waterproof stone paint emulsion.

[0016] Compared with the prior art, the waterproof stone paint emulsion composition and its preparation method of the present invention have the following beneficial effects:

[0017] The waterproof stone-like paint emulsion composition of the present invention includes butyl acrylate, functional monomers, mixed monomers, acrylic monomers, crosslinking monomers, organosilicon monomers, initiators, emulsifiers, and deionized water. The combined use of butyl acrylate and acrylic monomers in the formulation system of the present invention enhances the low-temperature resistance of the emulsion after film formation, and their relatively soft properties help the emulsion form a better film, thereby improving waterproof performance. The addition of organosilicon monomers can improve the waterproof performance of the coating and reduce the phenomenon of water absorption and whitening of the coating. Crosslinking monomers, through crosslinking reactions with other monomers, form a three-dimensional network structure, thereby improving the water resistance of the coating. The waterproof stone-like paint emulsion formulation system of the present invention exhibits the synergistic effect of various monomers and additives, as well as the stability and uniformity of the emulsion system. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0019] Example 1

[0020] A waterproof stone paint emulsion composition comprises 80.5 kg of butyl acrylate, 25 kg of functional monomers, 0.25 kg of mixed monomers, 0.4 kg of acrylic monomers, 0.3 kg of crosslinking monomers, 0.4 kg of organosilicon monomers, 0.55 kg of initiator, 0.9 kg of emulsifier, and 85 kg of deionized water.

[0021] Furthermore, the functional monomer in the waterproof stone paint emulsion composition of this embodiment is acrylamide.

[0022] Furthermore, the mixed monomer components and their mass percentages in the waterproof stone paint emulsion composition of this embodiment are: 45% aromatic unsaturated monomers, 25% acrylate unsaturated monomers and 30% carboxyl-containing unsaturated monomers.

[0023] Furthermore, in this embodiment, the acrylic acid in the waterproof stone paint emulsion composition is acrylic acid.

[0024] Furthermore, in this embodiment, the crosslinking monomer in the waterproof stone paint emulsion composition is a mixture of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate, wherein the mass ratio of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate is 3:1.

[0025] Furthermore, the organosilicon monomer in the waterproof stone paint emulsion composition of this embodiment is γ-methacryloyloxypropyltrimethylsilane.

[0026] Furthermore, the initiator in the waterproof stone paint emulsion composition of this embodiment is potassium persulfate.

[0027] Furthermore, in this embodiment, the emulsifier in the waterproof stone paint emulsion composition is polyoxyethylene sorbitan fatty acid ester.

[0028] According to the above formula, the preparation method of the waterproof stone paint emulsion of this embodiment includes the following steps:

[0029] Step 1: Add emulsifier and deionized water to the emulsification tank and stir at high speed. After the emulsifier is completely dissolved, add crosslinking monomer and pre-emulsify at high speed for 20 minutes to obtain pre-emulsion. Take out 5% as seed pre-emulsion for later use.

[0030] Step 2: After adding butyl acrylate, functional monomers, mixed monomers, and acrylic monomers to the reactor, the temperature is raised. When the temperature reaches 83°C, the seed pre-emulsion from Step 1 is added. After 2 minutes, the initiator is added, and the pre-emulsion from Step 1 is continuously added dropwise for 1.5 hours. When the remaining amount of the pre-emulsion from Step 1 is 20%, organosilicon monomers are added to the reactor and mixed and added dropwise for 1.5 hours. After the addition is completed, the temperature is maintained for 1 hour, then lowered to 75°C and maintained for 30 minutes. Subsequently, the temperature is lowered, and the pH of the emulsion is adjusted to 8.0 to obtain the waterproof stone paint emulsion.

[0031] Example 2

[0032] A waterproof stone paint emulsion composition comprises 71.5 kg of butyl acrylate, 20 kg of functional monomers, 0.2 kg of mixed monomers, 0.3 kg of acrylic monomers, 0.2 kg of crosslinking monomers, 0.3 kg of organosilicon monomers, 0.5 kg of initiator, 0.7 kg of emulsifier, and 70 kg of deionized water.

[0033] Furthermore, in this embodiment, the functional monomer in the waterproof stone paint emulsion composition is methyl acrylate monomer.

[0034] Furthermore, the mixed monomer components and their mass percentages in the waterproof stone paint emulsion composition of this embodiment are: 55% aromatic unsaturated monomers, 10% acrylate unsaturated monomers and 35% carboxyl-containing unsaturated monomers.

[0035] Furthermore, in this embodiment, the acrylic acid in the waterproof stone paint emulsion composition is methacrylic acid.

[0036] Furthermore, in this embodiment, the crosslinking monomer in the waterproof stone paint emulsion composition is a mixture of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate, wherein the mass ratio of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate is 1:1.

[0037] Furthermore, in this embodiment, the organosilicon monomer in the waterproof stone paint emulsion composition is polydimethylsiloxane methacrylate.

[0038] Furthermore, in this embodiment, the initiator in the waterproof stone paint emulsion composition is ammonium persulfate.

[0039] Furthermore, in this embodiment, the emulsifier in the waterproof stone paint emulsion composition is fatty alcohol polyoxyethylene ether.

[0040] According to the above formula, the preparation method of the waterproof stone paint emulsion of this embodiment includes the following steps:

[0041] Step 1: Add emulsifier and deionized water to the emulsification tank and stir at high speed. After the emulsifier is completely dissolved, add crosslinking monomer and pre-emulsify at high speed for 10 minutes to obtain pre-emulsion. Take out 5% as seed pre-emulsion for later use.

[0042] Step 2: After adding butyl acrylate, functional monomers, mixed monomers, and acrylic monomers to the reactor, the temperature is raised. When the temperature reaches 82°C, the seed pre-emulsion from Step 1 is added. After 3 minutes, the initiator is added, and the pre-emulsion from Step 1 is continuously added dropwise for 2 hours. When the remaining amount of the pre-emulsion from Step 1 is 15%, organosilicon monomers are added to the reactor and mixed and added dropwise for 2 hours. After the addition is completed, the temperature is maintained for 1 hour, then cooled to 70°C and maintained for 40 minutes. Subsequently, the temperature is lowered, and the pH of the emulsion is adjusted to 8.0 to obtain the waterproof stone paint emulsion.

[0043] Example 3

[0044] A waterproof stone paint emulsion composition comprises 89.5 kg of butyl acrylate, 30 kg of functional monomers, 0.3 kg of mixed monomers, 0.5 kg of acrylic monomers, 0.4 kg of crosslinking monomers, 0.5 kg of organosilicon monomers, 0.6 kg of initiator, 1.1 kg of emulsifier, and 100 kg of deionized water.

[0045] Furthermore, the functional monomer in the waterproof stone paint emulsion composition of this embodiment is N,N-methylenebisvinylamide.

[0046] Furthermore, the mixed monomer components and their mass percentages in the waterproof stone paint emulsion composition of this embodiment are: 35% aromatic unsaturated monomers, 30% acrylate unsaturated monomers and 35% carboxyl-containing unsaturated monomers.

[0047] Furthermore, in this embodiment, the acrylic acid in the waterproof stone paint emulsion composition is a mixture of acrylic acid and methacrylic acid, wherein the mass ratio of acrylic acid to methacrylic acid is 1:1.

[0048] Furthermore, in this embodiment, the crosslinking monomer in the waterproof stone paint emulsion composition is a mixture of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate, wherein the mass ratio of N-hydroxymethylacrylamide or N-(2-hydroxyethyl)acrylamide and glycidyl methacrylate is 5:1.

[0049] Furthermore, in this embodiment, the organosilicon monomer in the waterproof stone paint emulsion composition is a mixture of γ-methacryloxypropyltrimethylsilane and polydimethylsiloxane methacrylate, wherein the mass ratio of γ-methacryloxypropyltrimethylsilane to polydimethylsiloxane methacrylate is 1:1.

[0050] Furthermore, in this embodiment, the initiator in the waterproof stone paint emulsion composition is sodium persulfate.

[0051] Furthermore, in this embodiment, the emulsifier in the waterproof stone paint emulsion composition is a mixture of polyoxyethylene sorbitan fatty acid ester and fatty alcohol polyoxyethylene ether, wherein the mass ratio of polyoxyethylene sorbitan fatty acid ester to fatty alcohol polyoxyethylene ether is 1:1.

[0052] According to the above formula, the preparation method of the waterproof stone paint emulsion of this embodiment includes the following steps:

[0053] Step 1: Add emulsifier and deionized water to the emulsification tank and stir at high speed. After the emulsifier is completely dissolved, add crosslinking monomer and pre-emulsify at high speed for 30 minutes to obtain pre-emulsion. Take out 5% as seed pre-emulsion for later use.

[0054] Step 2: After adding butyl acrylate, functional monomers, mixed monomers, and acrylic monomers to the reactor, the temperature is raised. When the temperature reaches 85°C, the seed pre-emulsion from Step 1 is added. After 1 minute, the initiator is added, and the pre-emulsion from Step 1 is continuously added dropwise for 1 hour. When the remaining amount of the pre-emulsion from Step 1 is 25%, organosilicon monomers are added to the reactor and mixed and added dropwise for 1 hour. After the addition is completed, the temperature is maintained for 1 hour, then cooled to 80°C and maintained for 20 minutes. Subsequently, the temperature is lowered, and the pH of the emulsion is adjusted to 8.0 to obtain the waterproof stone paint emulsion.

[0055] Comparative Example 1

[0056] The ingredients in Example 1, "80.5 kg of butyl acrylate, 25 kg of functional monomers, 0.25 kg of mixed monomers, 0.4 kg of acrylic monomers, 0.3 kg of crosslinking monomers, 0.4 kg of organosilicon monomers, 0.55 kg of initiator, 0.9 kg of emulsifier, and 85 kg of deionized water", are changed to "80.9 kg of butyl acrylate, 25 kg of functional monomers, 0.25 kg of mixed monomers, 0.3 kg of crosslinking monomers, 0.4 kg of organosilicon monomers, 0.55 kg of initiator, 0.9 kg of emulsifier, and 85 kg of deionized water", and the rest of the operation is the same as in Example 1.

[0057] Test case

[0058] The emulsion stability, appearance, and water resistance of the waterproof stone paint emulsions prepared in Examples 1-3 and Comparative Example 1 were tested according to standard JG / T 24—2018. The test results are shown in Table 1 below:

[0059] Table 1

[0060]

[0061] The above description is merely an embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of the present invention should be included within the scope of the claims of the present invention.

Claims

1. A waterproof real stone paint emulsion composition, It is characterized in that The invention comprises, by weight, 71.5-89.5 parts of butyl acrylate, 20-30 parts of functional monomers, 0.2-0.3 parts of mixed monomers, 0.3-0.5 parts of acrylic acid monomers, 0.2-0.4 parts of cross-linking monomers, 0.3-0.5 parts of organosilicon monomers, 0.5-0.6 parts of initiators, 0.7-1.1 parts of emulsifiers and 70-100 parts of deionized water.

2. A waterproof true stone paint emulsion composition according to claim 1, It is characterized in that The functional monomer is at least one of acrylamide, methyl acrylate and N,N-methylenebisvinylamide.

3. A waterproof true stone paint emulsion composition according to claim 1, It is characterized in that The mixed monomer components and their mass percentages are: 35-55% of aromatic unsaturated monomers, 10-30% of acrylic ester unsaturated monomers and 25-40% of carboxyl-containing unsaturated monomers.

4. A waterproof true stone paint emulsion composition according to claim 1, It is characterized in that The acrylic acid is at least one of acrylic acid and methacrylic acid.

5. A waterproof real stone paint emulsion composition according to claim 1, It is characterized in that The crosslinking monomer is a mixture of N-hydroxymethyl acrylamide or N-(2-hydroxyethyl) acrylamide and glycidyl methacrylate, wherein the mass ratio of N-hydroxymethyl acrylamide or N-(2-hydroxyethyl) acrylamide to glycidyl methacrylate is (1-5):

1.

6. A waterproof real stone paint emulsion composition according to claim 1, It is characterized in that The organic silicon monomer is at least one of γ-methacryloxypropyltrimethylsilane and polydimethylsiloxy methacrylate.

7. A waterproof real stone paint emulsion composition according to claim 1, It is characterized in that The initiator is at least one of potassium persulfate, ammonium persulfate and sodium persulfate.

8. A waterproof real stone paint emulsion composition according to claim 1, It is characterized in that The emulsifier is at least one of polyoxyethylene sorbitan fatty acid ester and fatty alcohol polyoxyethylene ether.

9. A method for preparing a waterproof true stone paint emulsion, It is characterized in that The following steps are involved: Step 1, add emulsifier and deionized water into an emulsifier kettle and stir at high speed, add crosslinking monomer after the emulsifier is completely dissolved, pre-emulsify at high speed for 10-30 minutes to obtain pre-emulsion, and take out 5% as seed pre-emulsion for standby use; Step 2, adding butyl acrylate, functional monomer, mixed monomer and acrylic monomer into the reaction kettle and then heating up, when the temperature rises to 82-85°C, adding the seed pre-emulsion in step 1, adding the initiator after 1-3 minutes and continuously dripping the pre-emulsion in step 1 for 1-2 hours, when the remaining amount of the pre-emulsion in step 1 is 15-25%, adding the organosilicon monomer into the reaction kettle and mixing and dripping for 1-2 hours, keeping warm for 1 hour after the dripping, cooling to 70-80°C, keeping warm for 20-40 minutes, then cooling down, adjusting the pH of the emulsion to 8.0 to obtain the waterproof real stone paint emulsion.