Palladium ion imprinted polymer Pd < 2 + >-IIP and preparation method of sensor thereof

By introducing DMAEMA and FA on the surface of magnetic microspheres and preparing palladium ion-blotting polymers using KH-570 coupling agent and initiator, the problem of insufficient adsorption performance of existing temperature-sensitive ion-blotting polymers is solved, and high adsorption is achieved Capacity and selectivity, suitable for the detection of palladium ions.

CN118930767AInactive Publication Date: 2024-11-12NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410975643.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing temperature-sensitive ion-blotting polymers have problems of selectivity and insufficient adsorption capacity when adsorbing polyvalent metal ions, and their preparation process is complicated and difficult to meet the needs of industrial applications.

Method used

Using the preparation method of palladium ion-blotting polymer Pd2+-IIP, dimethylaminoethyl methacrylate (DMAEMA) and biochemical chlorhexidine (FA) are introduced on the surface of the magnetic microspheres Fe3O4/SiO2, and coupling is carried out using KH-570 silane. The agent and ammonium persulfate sodium bisulfite initiator form a water-in-oil emulsion. After nitrogen deoxygenation and silane coupling reaction, the template ions are removed, and palladium ion-blotting polymer with high adsorption properties is prepared and the Modified onto the glassy carbon electrode to form a palladium ion-blot polymer sensor.

Benefits of technology

The specific surface area, pore volume and average pore size of the palladium ion-blotting polymer are improved, the adsorption performance of template ions is enhanced, and the high selectivity detection of palladium ions is achieved. The preparation process is relatively simple, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930767A_ABST
    Figure CN118930767A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a palladium ion imprinted polymer Pd < 2 + >-IIP and a sensor thereof, and belongs to the field of electrochemical synthesis. The preparation method comprises the following steps: putting cyclohexane and Span 80 into a three-neck flask, uniformly stirring to form an oil phase, taking acrylamide, dimethylaminoethyl methacrylate, sodium tetrachloropalladate, biochemical fulvic acid and magnetic microspheres, adding deionized water into a beaker, ultrasonically dispersing uniformly to form a water phase, pouring the water phase into the three-neck flask to form a water-in-oil emulsion, and introducing nitrogen to remove oxygen; dropwise adding a composite initiator solution prepared from ammonium sulfate and sodium hydrogen sulfite; then, dropwise adding a silane coupling agent, repeatedly washing the obtained product with deionized water and absolute ethyl alcohol for multiple times, then removing palladium ions in the polymer with a diluted hydrochloric acid solution until supernate is neutral and the palladium ions cannot be detected through a color developing agent, and drying to obtain Pd < 2 + >-IIP. Compared with a nonionic imprinted polymer, the specific surface area, the pore volume and the average pore size of the product are all larger than those of the nonionic imprinted polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a palladium ion imprinted polymer Pd 2+ The invention relates to a preparation method of an IIP and a palladium ion imprinted polymer sensor, and belongs to the field of electrochemical synthesis. Background Art

[0002] Thermosensitive ion-imprinted polymer is a new type of intelligent adsorption material with the advantages of convenient separation, low cost, good selective recognition performance, etc., and its adsorption performance for multivalent metal ions can be affected by changing the adsorption temperature, and it has gradually become a research hotspot. Using magnetic microspheres as the matrix, biochemical humic acid (FA) and thermosensitive monomer dimethylaminoethyl methacrylate (DMAEMA) were introduced, and Pd (II) was used as the template ion to prepare a new type of palladium ion-imprinted polymer with simple separation operation, good selectivity, high adsorption capacity and temperature sensitivity, which has broad market prospects and value. Summary of the invention

[0003] To solve the above problems, the present invention adopts the following technical solutions:

[0004] A palladium ion imprinted polymer Pd 2+ -A method for preparing IIP, comprising the following steps:

[0005] Put 40mL cyclohexane and 2mL Span 80 in a three-necked flask, stir evenly to form an oil phase, take 1.0g acrylamide AM, 1-5mmol temperature-sensitive functional monomer dimethylaminoethyl methacrylate DMAEMA, 0.02-0.07mg sodium tetrachloropalladate Na2PdCl4, 0.03g biochemical humic acid, 0.2-0.6g magnetic microspheres, add deionized water in a beaker, ultrasonically disperse evenly to form an aqueous phase, pour into a three-necked flask to form an oil-in-water emulsion, and pass nitrogen to deoxygenate;

[0006] Add dropwise a composite initiator solution prepared by mixing 50-200 mg of ammonium persulfate and sodium bisulfite in a mass ratio of 1:1;

[0007] Then, KH-570 silane coupling agent was added dropwise, and the obtained product was repeatedly washed with deionized water and anhydrous ethanol for several times, and then the palladium ions in the polymer were removed with a 0.5 mol / L dilute hydrochloric acid solution until the supernatant was neutral and no palladium ions were detected by the developer, and the product was dried in a vacuum drying oven for 12 h to obtain the palladium ion imprinted polymer Pd 2+ -IIP.

[0008] Furthermore, the amount of the KH-570 coupling agent used is 2.0 mL, the amount of sodium tetrachloropalladate Na2PdCl4 used is 0.05 g, the amount of magnetic microspheres Fe3O4 / SiO2 used is 0.40 g, the amount of functional monomer DMAEMA used is 3 mmol, the reaction temperature is 40°C, and the reaction time is 8 h.

[0009] Furthermore, the preparation method of the magnetic microspheres Fe3O4 / SiO2 is as follows: prepare magnetic Fe3O4 by coprecipitation method, weigh 0.50g Fe3O4 and 1.0g hexadecyltrimethylammonium bromide CTAB in a beaker, add 20mL deionized water and 200mL anhydrous ethanol, and disperse evenly by ultrasonication, transfer to a three-necked flask and stir for 30min, add 3mL tetraethyl orthosilicate TEOS, add 4-7mL ammonia water dropwise at 30°C, stir and react for 24h, after the reaction is completed, wash the separated sample repeatedly with anhydrous ethanol and deionized water several times, and place it in a vacuum drying oven to dry for 24h. The product is placed in a muffle furnace, roasted at 550°C for 6h, and the magnetic microspheres Fe3O4 / SiO2 are obtained after cooling.

[0010] A method for preparing a palladium ion imprinted polymer sensor, wherein the preparation process comprises the following steps:

[0011] First, the glassy carbon electrode GCE with a diameter of 3 mm was pretreated by polishing the surface of the glassy carbon electrode with alumina powder with a particle size of 0.3 μm and 0.5 μm, respectively, and repeatedly rinsed with anhydrous ethanol and deionized water, and ultrasonically washed in an ultrasonic cleaner for 3 minutes, and the operation was repeated several times to remove the powder remaining on the surface of the glassy carbon electrode after polishing, and dried with nitrogen to prevent oxidation, and activated with a 0.5 mol / L dilute sulfuric acid solution;

[0012] Then 0.05 g of palladium ion-imprinted polymer Pd 2+ -IIP, anhydrous ethanol and Nafion perfluorinated resin solution were mixed and ultrasonicated for 30 minutes to form a uniform suspension, which was evenly dropped onto the surface of the activated glassy carbon electrode. After the ethanol evaporated at room temperature, a film was formed on the electrode surface, thus preparing a palladium ion imprinted polymer sensor.

[0013] Beneficial effects of the present invention: Compared with non-ionic imprinted polymers, the specific surface area, pore volume and average pore size of palladium ion imprinted polymers are larger than those of non-ionic imprinted polymers. The main reason is that during the synthesis of the polymer, palladium ion imprinted pores are formed in the polymer after the template ions are removed, resulting in an increase in pore volume, specific surface area and average pore size, which is beneficial to improving the specific surface area of ​​palladium ion imprinted polymers for template ions Pd 2+ The palladium ion imprinted polymer sensor has good selectivity for template ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 Effect of silane coupling agent KH-570 on adsorption performance

[0015] Figure 2 Effect of the dosage of Na2PdCl4 on Pd 2+ -IIP adsorption performance

[0016] Figure 3 Effect of the dosage of magnetic microspheres (Fe3O4 / SiO2) on adsorption performance

[0017] Figure 4 Effect of DMAEMA on adsorption performance

[0018] Figure 5 Effect of reaction temperature on Pd 2+ -IIP adsorption performance

[0019] Figure 6 Effect of reaction time on adsorption performance

[0020] Figure 7 Fe3O4 / SiO2, FA, Pd 2+ -Infrared spectrum of IIP

[0021] Figure 8 Fe3O4, Fe3O4 / SiO2, Pd 2+ -XRD diffraction patterns of IIP and NIP

[0022] Fig. 9 Fe3O4 / SiO2, NIP, Pd 2+ -SEM image of IIP

[0023] Fig.10 Fe3O4 / SiO2, Pd 2+ -Thermogravimetric analysis curve of IIP

[0024] Fig.11 NIP and Pd 2+ -N2 adsorption-desorption isotherms and pore size distribution of IIP

[0025] Fig.12 (A) Relationship between deposition voltage and peak current; (B) Relationship between deposition time and current

[0026] Fig.13 Relationship curve between adsorption time and electrochemical signal of Pd(II) detected by sensor

[0027] Fig.14 The electrochemical response curve of Pd(II) to the molar ratio of template ion to functional monomer

[0028] Fig.15 (A) DPASV curves of different concentrations of Pd(II) (pH=5.0), from a to i, the concentrations are 0.5, 1, 5, 10, 15, 35, 80, 100 μM; (B) Peak current corresponding to Pd(II) concentration curve

[0029] Fig.16 Repeatability of electrochemical sensors

[0030] Fig.17 Schematic diagram of the preparation of magnetic microspheres. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below through examples and comparative examples.

[0032] Example 1: Preparation of palladium ion imprinted polymer Pd 2+ -IIP

[0033] refer to Figure 1 Sodium tetrachloropalladate (Na2PdCl4) was used as the template ion Pd(II) source, dimethylaminoethyl methacrylate (DMAEMA) was used as the thermosensitive functional monomer, and fulvic acid (FA) was introduced. Under the action of KH-570 silane coupling agent, the polymer was loaded onto the surface of magnetic microspheres (Fe3O4 / SiO2). The optimal preparation conditions of palladium ion imprinted polymer were optimized by single factor method. 1) Effect of the dosage of KH-570 coupling agent on adsorption performance

[0034] In order to introduce easily polymerizable double bonds on the surface of magnetic microspheres (Fe3O4 / SiO2), KH-570 was used as a silane coupling agent. The siloxymethyl groups in the molecular structure of KH-570 and the silanol groups on the surface of the magnetic microspheres form a Si-O-Si structure, and the double bonds in the molecular structure of KH-570 can be copolymerized with acrylamide (AM) and dimethylaminoethyl methacrylate (DMAEMA).

[0035] Weigh 0.05g of sodium tetrachloropalladate (Na2PdCl4), 0.30g of biochemical humic acid (FA), add appropriate amount of deionized water to form a mixed solution, weigh 0.40g of magnetic microspheres (Fe3O4 / SiO2), keep other conditions unchanged, the reaction temperature is 40℃, nitrogen is passed through to deoxygenate, and then the composite initiator is added to react for 8h. The amount of KH-570 coupling agent is changed to 1.0mL, 1.5mL, 2.0mL, 2.5mL, and 3.0mL respectively. Select 10mg sample, 20mL 100mg / L Pd 2+ The aqueous solution was shaken at a constant temperature of 45°C for 6 hours, and the supernatant was measured under the action of an external magnetic field to detect the equilibrium adsorption of palladium ions by the ion-imprinted polymer. The adsorption results are shown in Figure 1The amount of KH-570 coupling agent can affect the Pd 2+ -IIP adsorption performance of palladium ions. With the increase of KH-570 coupling agent dosage, Pd 2+ -IIP's adsorption of palladium ions first increases and then decreases. When the dosage of KH-570 coupling agent is 2.0 mL, the maximum saturated adsorption amount is 81.05 mg / g. Ionic bonds and hydrogen bonds are formed between humic acid molecules and copolymer molecules. Therefore, the introduction of KH-570 molecules makes the organic polymer layer and the inorganic magnetic core chemically bonded, which is not easy to fall off. When a small amount of KH-570 molecules are added, acrylamide and dimethylaminoethyl methacrylate cannot fully undergo ternary copolymerization with the double bonds in the KH-570 molecules. Most of the adsorption is carried out by homopolymerization or copolymerization of acrylamide and dimethylaminoethyl methacrylate. The homopolymerization or copolymer of acrylamide and dimethylaminoethyl methacrylate and humic acid macromolecules are easily eluted from the Fe3O4 / SiO2 surface, resulting in less organic polymer layer on the Fe3O4 / SiO2 surface, so the adsorption of Pd 2+ Effective adsorption cannot be performed. When the amount of KH-570 is too much, the silyl methoxy groups in the molecular structure of KH-570 react to form a Si-O-Si structure, which plays a cross-linking role and causes the hydrophilicity of the organic layer to deteriorate. Therefore, within the experimental range, when KH-570 is 2.0 mL, it not only improves the stability between the organic layer and the inorganic magnetic core, but also plays a certain cross-linking role, improves the stability of the imprinted hole, and thus the saturated adsorption amount increases. Therefore, the optimal amount of KH-570 coupling agent selected in the experiment is 2.0 mL.

[0036] 2) Effect of the dosage of Na2PdCl4 on adsorption performance

[0037] The amount of template ions will also affect the adsorption performance of the final product to template ions. The amount of KH-570 silane coupling agent was fixed at 2.0 mL, and the amount of sodium tetrachloropalladate (Na2PdCl4) was changed. 0.02g, 0.03g, 0.04g, 0.05g, 0.06g and 0.07g Na2PdCl4 were added respectively to prepare palladium ion imprinted polymers, and other conditions were kept unchanged. The experimental results obtained are shown in Figure 2 It can be seen that with the increase of Na2PdCl4 in the synthesis reaction system, Pd 2+ The saturated adsorption of palladium ions by the synthesized ion-imprinted polymer first increased and then decreased. Within the experimental range, when the added sodium tetrachloropalladate was 0.02 g, the adsorption of palladium ions by the polymer was at least 52.43 mg / g. 2+With the increase of concentration, the saturated adsorption capacity of the imprinted polymer gradually increases. When the added amount is 0.05g, the saturated adsorption capacity of the ion-imprinted polymer for the template ion reaches a maximum value of 81.05mg / g. Continuing to increase the dosage of Na2PdCl4, the saturated adsorption capacity of the ion-imprinted polymer gradually decreases. The main reason is that when too few template ions are added to the system, the imprinted holes formed by the imprinted polymer will also be relatively small, so the saturated adsorption capacity is also small; when excessive template ions are added, there are too many imprinted holes in the imprinted polymer, and there are fewer binding sites between the template ions and the organic polymer, which not only affects the stability of the imprinted holes, but also the adsorption capacity is insufficient when encountering the template ions again. Therefore, the optimal amount of Na2PdCl4 added to prepare the ion-imprinted polymer is 0.05g, at which time the adsorption performance is the best.

[0038] 3) Effect of the dosage of magnetic microspheres (Fe3O4 / SiO2) on adsorption performance

[0039] Magnetic microspheres (Fe3O4 / SiO2) are important matrix materials for the preparation of ion-imprinted polymer systems. The dosage of silane coupling agent KH-570 was selected as 2.0 mL, the dosage of sodium tetrachloropalladate (Na2PdCl4) was selected as 0.05 g, the dosage of magnetic microspheres was changed, and 0.20 g, 0.30 g, 0.40 g, 0.50 g, and 0.60 g were added to the system respectively. Other conditions remained unchanged, and the adsorption performance of the final product on palladium ions was tested respectively. The experimental results are shown in Figure 3 It can be seen that with the increase in the amount of magnetic microspheres, the adsorption of palladium ions by the ion-imprinted polymer also increases. When 0.40g of magnetic microspheres are added to the system, the adsorption of palladium ions by the imprinted polymer is the best. However, when the dosage continues to increase, the adsorption of template ions by the ion-imprinted polymer decreases rapidly. The main reason is that when the functional monomer and other conditions are certain, there are fewer magnetic microspheres, resulting in no or fewer magnetic microspheres inside the formed imprinted polymer, resulting in a thicker organic polymer layer, the deep imprinted holes are covered, and the adsorption effect cannot be fully exerted; when there are too many magnetic microspheres, the imprinted polymer is wrapped too thinly on its surface, the number of organic imprinted holes per unit mass is small, and the saturated adsorption amount is reduced. Therefore, the optimal dosage of magnetic microspheres (Fe3O4 / SiO2) in the system is 0.40g, and the prepared ion-imprinted polymer has the best adsorption of palladium ions.

[0040] 4) Effect of functional monomer dosage on adsorption performance

[0041] Functional monomer dimethylaminoethyl methacrylate (DMAEMA) is one of the key substances for preparing ion-imprinted polymers. The active functional groups in DMAEMA can react with the template ions Pd 2+Chelation, after removing the template ions, imprinted holes are formed. Therefore, the amount of functional monomer can affect the adsorption performance of ion-imprinted materials to target ions. The experiment selected the amount of silane coupling agent as 2.0mL, the amount of sodium tetrachloropalladate as 0.05g, the reaction temperature as 40℃, and only the amount of thermosensitive functional monomer (DMAEMA) was changed. The amount of DMAEMA was weighed as 1mmol, 2mmol, 3mmol, 4mmol, and 5mmol respectively. The other conditions remained unchanged. The ion-imprinted polymers prepared with different amounts of functional monomers were studied for the adsorption of template ions Pd 2+ The adsorption performance of Figure 4 It can be seen that the amount of the thermosensitive functional monomer DMAEMA added during the reaction has a great influence on the adsorption properties of the final product. With the increase of the amount of the functional monomer, the ion-imprinted polymer has a greater effect on the adsorption of the template ion Pd 2+ The saturated adsorption capacity of the ion-imprinted polymer increases first and then decreases. In the range of 1-3 mmol, with the increase of the amount of the functional monomer DMAEMA, the saturated adsorption capacity of the ion-imprinted polymer for palladium ions gradually increases. When the amount of DMAEMA is 3 mmol, the maximum saturated adsorption capacity of the prepared ion-imprinted polymer for palladium ions is 81.05 mg / g. With the further increase of the amount of DMAEMA, the saturated adsorption capacity decreases. The main reason may be that in the reaction system, the amount of crosslinker and initiator is certain. When the amount of functional monomer is low, the final prepared ion-imprinted polymer does not produce enough imprinted holes. Gradually increasing the amount of functional monomer will increase the number of imprinted holes in the product, resulting in an increase in the saturated adsorption capacity of the ion-imprinted polymer. When the amount of functional monomer is excessive, a part of the thermosensitive monomer self-polymerizes excessively, which makes the functional monomer actually participating in the synthesis of the ion-imprinted polymer decrease or the template ions are buried too deeply in the polymer and cannot be eluted, and the imprinted holes cannot be formed, resulting in a decrease in the adsorption capacity of the ion-imprinted polymer for the template ions. Therefore, the optimal amount of the functional monomer DMAEMA in the preparation of ion-imprinted polymer is 3 mmol.

[0042] 5) Effect of reaction temperature on adsorption performance

[0043] The temperature of the reaction system can affect the synthesis of ion-imprinted polymers to a certain extent, thereby affecting their adsorption performance for palladium ions. The experiment selected the dosage of KH-570 silane coupling agent as 2.0 mL and the dosage of sodium tetrachloropalladate as 0.05 g. Only the temperature of the reaction system was changed, and the reaction temperature was set to 25°C, 30°C, 35°C, 40°C, 45°C and 50°C respectively. The other conditions remained unchanged. The adsorption performance of ion-imprinted polymers prepared at different temperatures for palladium ions was studied. The experimental results are shown in Figure 5It can be seen that the reaction temperature has a great influence on the adsorption properties of the final product. With the increase of temperature, the adsorption of palladium ions by the ion-imprinted polymer first increases and then decreases. In the range of 25-40°C, with the increase of the temperature of the reaction system, the adsorption of palladium ions by the ion-imprinted polymer increases rapidly. When the temperature is raised to 40°C, the maximum adsorption of palladium ions by the prepared imprinted polymer is 81.05 mg / g. When the temperature continues to rise, the adsorption of palladium ions decreases rapidly. The main reason is that when the temperature is low, the decomposition rate of the initiator is slow, and the free radicals generated by the decomposition are less, so less polymer is generated in the system and it is impossible to form enough imprinted holes. Therefore, the ion-imprinted polymer has a low adsorption rate for Pd 2+ The saturated adsorption capacity is low; when the temperature rises to 40℃, the initiator has an appropriate decomposition rate, produces enough free radicals, promotes the polymerization reaction between monomers, and enables the imprinted polymer to be evenly attached to the surface of the magnetic microspheres (Fe3O4 / SiO2); when the temperature is too high, the thermal decomposition rate of the initiator is too fast, which increases the self-crosslinking rate of the monomer and the KH-570 coupling agent, and reduces the actual monomer and KH-570 involved in the reaction, which affects the formation of imprinted holes in the ion-imprinted polymer, resulting in the ion-imprinted polymer to Pd 2+ The saturated adsorption capacity of ion-imprinted polymer was reduced. Therefore, the optimal reaction temperature for preparing ion-imprinted polymer was 40℃.

[0044] 6) Effect of reaction time on adsorption performance

[0045] The length of reaction time will affect the formation of ion-imprinted polymer, thus making the adsorption effect of ion-imprinted polymer on template ions unsatisfactory. The amount of cross-linking agent KH-570 was selected as 2.0 mL, the reaction temperature was 40 ° C, and only the length of reaction time was changed to 5h, 6h, 7h, 8h, 9h and 10h respectively. Other conditions remained unchanged. The adsorption performance of the final product on palladium ions is shown in Figure 6 It can be seen that as the polymerization reaction time in the reaction system increases, the adsorption amount of palladium ions by the palladium ion imprinted polymer increases until there is almost no significant change. Within 5 to 8 hours, as time increases, the final equilibrium adsorption amount reaches a maximum value of 81.05 mg / g. After more than 8 hours, the change in adsorption amount is almost negligible. The main reason is that as the polymerization reaction proceeds, the functional monomers and other raw materials in the system are continuously consumed to form ion-imprinted polymers coated on the surface of the magnetic microspheres. After a certain time point, the reaction in the system reaches equilibrium and no polymer is formed. After the template ions are eluted, the ion-imprinted holes formed in the product no longer increase. Even if the reaction time is extended, the adsorption performance of the obtained ion-imprinted polymer for the template ions will not change significantly. Therefore, the optimal reaction time for preparing ion-imprinted polymers in the experiment is 8 hours.

[0046] Infrared spectroscopy

[0047] The potassium bromide tableting method was used to 2+ -IIP infrared spectroscopy analysis, the results are shown in Figure 7 It can be seen that in the spectrum of Fe3O4 / SiO2, 3450cm -1 The stretching vibration peak of -OH appears nearby, 1625 cm -1 The nearby peak is the bending vibration peak of -OH, 1100cm -1 The peak of Si-O-Si stretching vibration is 470 cm -1 The stretching vibration peak of Fe-O is at 3390cm-1. -1 The C=C skeleton vibration of the aromatic ring is at 1410 cm -1 The peak at 3450cm is the bending vibration peak of -CH2. Compared with the FA and Fe3O4 / SiO2 spectra, -1 The vibration peak intensity of -OH at 2950cm-1 was significantly reduced because the Si-OH on the Fe3O4 / SiO2 magnetic microspheres was consumed during the modification process. -1 The peak of CH vibration of saturated aromatic hydrocarbons is 1719 cm -1 The stretching vibration peak of C=O of ester appears at 1463cm -1 The peak at the center is the CN stretching vibration peak in the amide, proving that the surface of the magnetic microspheres is covered with an ion-imprinted polymer layer.

[0048] X-ray diffraction analysis

[0049] XRD was used to characterize Fe3O4, Fe3O4 / SiO2, Pd 2+ -IIP, NIP and other materials were used for crystal structure characterization. The results are shown in Figure 8 It can be seen that Fe3O4 / SiO2, Pd 2+ The main diffraction peaks in the X-ray diffraction patterns of -IIP and NIP are consistent with the characteristic diffraction peaks of standard magnetic Fe3O4, which is a trans-spinel structure and belongs to the cubic crystal system. This proves that the magnetic core has always existed during the reaction. After removing the template ions, no other diffraction peaks appeared, indicating that palladium ion imprinting holes were formed inside the polymer, and Pd was successfully prepared. 2+ -IIP, and Pd 2+ The main diffraction peak of -IIP is the same as that of Fe3O4, indicating that after Fe3O4 is wrapped layer by layer, its crystal form does not change and retains strong paramagnetism.

[0050] Scanning electron microscopy analysis

[0051] Scanning electron microscopy was used to investigate the magnetic microspheres (Fe3O4 / SiO2), nonionic imprinted polymers (NIP) and ionic imprinted polymers (Pd 2+ -IIP) particles were analyzed for apparent morphology, and the results are shown in Fig. 9 It can be seen that (a) and (b) are surface morphology images of Fe3O4 / SiO2 at different magnifications, and the morphology structure is a spherical particle with uniform particles, which can preliminarily prove the successful preparation of magnetic nanoparticles. Figure 7 (c) and (d) are the morphological structures of nonionic imprinted polymers (NIP). Figure 7 (e) and (f) are palladium ion imprinted polymers (Pd 2+ -IIP) morphology and structure diagram. It can be seen from the figure that Pd 2+ -IIP and NIP particle sizes are significantly larger than those of magnetic microspheres Fe3O4 / SiO2, indicating that the polymer is successfully coated on the surface of the magnetic microspheres; NIP and Pd 2+ -IIP compared to Pd 2+ The particle size of -IIP is slightly larger than that of NIP. The main reason is that after the polymerization reaction, a template ion eluent is needed to remove the template ions in the polymer, resulting in the formation of a large number of imprinted pores.

[0052] Thermogravimetric analysis

[0053] Magnetic microspheres (Fe3O4 / SiO2) and Pd 2+ -IIP was subjected to thermogravimetric analysis, the results are shown in Fig.10 It can be seen that Fe3O4 / SiO2 and Pd 2+ Compared with the thermogravimetric curve of -IIP, the latter has a more obvious decline, which is caused by the thermal decomposition of the polymer layer wrapped on the surface of the magnetic microspheres. 2+ -IIP weight loss rates were about 1.24% and 2.05%, respectively, mainly due to the evaporation of water on the sample surface. After the temperature continued to rise, the weight loss rate of Fe3O4 / SiO2 slowly decreased, because the Si-OH therein gradually dehydrated to become a Si-O-Si structure. After the temperature reached 780°C, the product no longer decomposed, and the weight loss rate was about 15.6%. Between 200 and 500°C, Pd 2+ -IIP has a faster weight loss rate, with a weight loss rate of about 25%, which is mainly caused by the rapid decomposition of the polymer layer on the surface of the microspheres at high temperatures. After that, the weight loss rate slows down, which is caused by the gradual dehydration of Si-OH in Fe3O4 / SiO2. From the above thermogravimetric analysis, it can be seen that Pd prepared with Fe3O4 / SiO2 as the magnetic core 2+ -IIP has a certain thermal stability.

[0054] N2 adsorption-desorption analysis

[0055] The surface area and pore size of ion-imprinted polymer and non-imprinted polymer were analyzed by N2 adsorption-desorption method. Fig.11 and Table 1.

[0056] Table 1 NIP and Pd 2+ -Specific surface area and pore structure parameters of IIP

[0057]

[0058] from Fig.11 It can be seen that the isotherms of non-imprinted materials and ion-imprinted materials conform to the type IV isotherms, indicating that there is a pore structure in the sample. At low pressure, the adsorption amount increases, mainly monolayer adsorption occurs. At high pressure, the isotherm increases sharply and an inflection point appears. A relatively obvious hysteresis loop appears in the figure, which is mainly due to the capillary condensation process. The hysteresis loop belongs to the H1 type, which is a uniform pore model, proving that the pore structure in the sample is ordered.

[0059] As shown in Table 1, non-imprinted polymer materials (NIP) and palladium ion imprinted polymers (Pd 2+ -IIP) are 451.69m 2 / g and 710.43m 2 / g, and the pore volume is 0.32cm 3 / g and 0.67cm 3 / g, and the average pore size was 2.43nm and 4.24nm, respectively. Compared with non-ionic imprinted polymers, the specific surface area, pore volume and average pore size of palladium ion imprinted polymers were larger than those of non-ionic imprinted polymers. The main reason is that during the synthesis of the polymer, palladium ion imprinted pores were formed in the polymer after the template ions were removed, resulting in an increase in pore volume, specific surface area and average pore size, which is beneficial to improve the specific surface area of ​​palladium ion imprinted polymers for template ions Pd 2+ adsorption performance.

[0060] Example 2: Preparation of palladium ion imprinted polymer sensor

[0061] The present invention modifies a palladium ion-imprinted polymer onto the surface of a glassy carbon electrode to form a working electrode, thereby preparing an ion-imprinted electrochemical sensor that can be used to detect palladium ions.

[0062] First, the glassy carbon electrode (GCE, diameter 3mm) was pretreated, and the surface of the glassy carbon electrode was polished with alumina powder with a particle size of 0.3μm and 0.5μm, respectively, and repeatedly rinsed with anhydrous ethanol and deionized water, and ultrasonically washed in an ultrasonic cleaner for 3min, and the operation was repeated several times to remove the powder remaining on the surface of the glassy carbon electrode after polishing. It was blown dry with nitrogen to prevent oxidation, and activated with 0.5mol / L dilute sulfuric acid solution. After 0.05g of ion-imprinted polymer, an appropriate amount of anhydrous ethanol and Nafion perfluorinated resin solution were mixed, ultrasonicated for 30min to form a uniform suspension, which was evenly dripped onto the surface of the activated glassy carbon electrode. After the ethanol evaporated at room temperature, a film was formed on the electrode surface, and a palladium ion-imprinted polymer sensor was prepared.

[0063] 1) Determination of deposition potential and deposition time

[0064] The electrochemical sensor composed of the palladium ion imprinted polymer modified working electrode was tested using deposition potential. The change of its peak current under different deposition potentials was shown in Fig.12 . As shown in Figure (A), with the increase of negative voltage, the corresponding peak current gradually increases. When the deposition potential reaches -0.8V, the corresponding current value reaches the maximum. As the potential continues to increase, the peak current decreases slightly and gradually stabilizes. Therefore, -0.8V is selected as the optimal deposition potential. The same method is used to explore the optimal deposition time. The results are shown in Figure (B). As time increases in the range of 50 to 180s, the peak current increases with time. As time continues to pass, at 180s, the peak current gradually becomes stable, indicating that the adsorption of the electrode surface has reached saturation. At this time, the thickness of the electrodeposited film is moderate, and palladium ions can easily reach the surface of the glassy carbon electrode through ion imprinting holes. After that, the deposition time continues to increase, and the peak current begins to decrease. It may be that as the thickness of the deposited film continues to increase, the palladium ions in the film cannot be completely eluted. Therefore, the optimal deposition time is selected as 180s.

[0065] 2) Effect of adsorption time on peak current of electrochemical sensor for detecting Pd(II)

[0066] Adsorption time is an influencing factor for the detection of palladium ions, which can affect the amount of palladium ions adsorbed by the palladium ion electrochemical sensor. By increasing the pre-adsorption time, a more sensitive electrochemical response signal can be obtained on the surface of the electrode material. In order to explore the effect of the adsorption time of the working electrode of the ion-imprinted material on the electrochemical response signal, the electrode material was placed in a 10 μmol / L Pd(II) solution, and the peak current at different adsorption times was measured. The results are shown in Figure 2. Fig.13It can be seen that with the continuous increase of time, the current response value is also increasing. When the adsorption time reaches 30 minutes, the maximum current value is 5.20μA. With the increase of adsorption time, the current changes slightly and basically tends to a stable state. The main reason is that when the adsorption time is too short, it may lead to insufficient combination between palladium ions and functional monomers, which is not conducive to the migration of electrons. After the adsorption time exceeds 30 minutes, the adsorption of the electrode material reaches saturation, so the current size no longer increases, indicating that the functional monomers in the palladium ion imprinted polymer on the surface of the glassy carbon electrode are fully combined with palladium ions, and the optimal adsorption time in the experiment is 30 minutes.

[0067] 3) Effect of the molar ratio of template ions to functional monomers on peak current

[0068] The number of binding sites between template ions and functional monomers in ion-imprinted polymers is mainly determined by the molar ratio of template ions to functional monomers. In order to explore the optimal electrochemical response signal of the sensor, five different ratios of imprinted polymer-modified glassy carbon electrodes with molar ratios of template ions to functional monomers = 1:1; 1:2; 1:3; 1:4; 1:5 were prepared, and electrochemical tests were carried out under the same other experimental conditions. The results are shown in Fig.14 It can be seen that when the molar ratio of template ions to functional monomers is between 1:1 and 1:3, the response current of the working electrode to palladium ions increases rapidly, and when it is between 1:3 and 1:5, it decreases rapidly. When the ratio is 1:3, the maximum response current of the working electrode is 13.51 μA. Therefore, when the molar ratio of template ions to functional monomers is 1:3, the effect is best.

[0069] 4) Standard curve and detection limit

[0070] After optimizing the experimental parameters, under the optimal test conditions (phosphate buffer solution with pH = 5.0, deposition potential -0.8V, pre-adsorption time 180s), the differential pulse voltammetry (DPASV) response curve of Pd(II) in the concentration range of 0.5 to 100 μM was measured using a palladium ion imprinted electrochemical sensor. The results are shown in Fig.15 . As shown in Figure (A), Pd(II) can be detected near -0.5V, and the peak current increases with the increase of Pd(II) concentration. As shown in Figure (B), the concentration of Pd(II) has a good linear relationship in the range of 0.5 to 50μM. According to the data fitting, the linear equation is Y = 0.4867x-0.3988 (R 2 =0.99), where Y is the peak current and x is the concentration of Pd(II). The detection limit was calculated according to formula (10), and the detection limit (LOD) of the palladium ion imprinted electrochemical sensor was 0.14 μM. In summary, the palladium ion imprinted electrochemical sensor has a wide linear range and a low detection limit.

[0071] 5) Ion imprinting selectivity

[0072] Selectivity is one of the important properties of ion imprinting sensors. In actual detection, the types of metal ions in water samples are relatively complex. Therefore, for electrochemical sensors, the template ions should have good selectivity. In order to investigate the selectivity of palladium ion imprinting electrochemical sensors for palladium ions, the effect of palladium ion imprinting polymer electrochemical sensors on the peak current of Pd(II) in the presence of different metal ions was detected. Ten times the concentration of different metal ions (Ni 2+ , K + , Fe 3+ , Pb 2+ , Ag + , Cu 2+ , Mn 2+ , Na + , Zn 2+ , Cd 2 + ), the change of the peak current is shown in Table 2. When no other metal ions are added, the peak current is 48.90μA. After adding interfering ions, the peak current changes. When the interfering ion is Ag, the peak current changes. + When the interfering ion is K + When , the peak current is 44.49μA, and the peak current decreases by 9%. This shows that when there is a certain concentration of interfering ions in the solution, the peak current changes slightly, the palladium ion imprinted electrochemical sensor still has a strong recognition ability for palladium ions, and the sensor has good selectivity.

[0073] Table 2 Effect of different metal ions on peak current

[0074]

[0075]

[0076] 6) Reusability

[0077] The prepared palladium ion imprinted electrochemical sensor was subjected to repeated adsorption-removal experiments in a phosphate buffer solution with a pH of 5 containing 100 μM Pd(II) for 7 cycles to evaluate its reusability. Fig.16It can be seen that when the experiment was repeated five times, the peak current of the ion-imprinted electrochemical sensor for Pd(II) changed only slightly. After five repetitions, the peak current decreased by 11.4%, and after seven repetitions, the peak current decreased by 24.6%. The main reason is that due to repeated adsorption-desorption experiments and long-term immersion in buffer solution, the polymer film on the surface of the glassy carbon electrode was damaged, causing the loss of palladium ion imprinted polymer, the number of palladium ion imprinted holes decreased, and the peak current of the palladium ion imprinted electrochemical sensor in response to palladium ions decreased. The experiment shows that the palladium ion imprinted electrochemical sensor has certain repeatability.

Claims

1. A palladium ion imprinted polymer Pd 2+ -A method for preparing IIP, characterized in that The following steps are involved: Put 40 mL cyclohexane and 2 mL Span 80 in a three-necked flask, stir evenly to form an oil phase, take 1.0 g acrylamide AM, 1-5 mmol thermosensitive functional monomer dimethylaminoethyl methacrylate DMAEMA, 0.02-0.07 mg sodium tetrachloropalladate Na2PdCl4, 0.03 g biochemical humic acid, 0.2-0.6 g magnetic microspheres, add deionized water in a beaker, ultrasonically disperse evenly to form an aqueous phase, pour into a three-necked flask to form an oil-in-water emulsion, and pass nitrogen to deoxygenate; A composite initiator solution prepared by 50-200 mg of ammonium persulfate and sodium bisulfite in a mass ratio of 1:1 was added dropwise; then, a KH-570 silane coupling agent was added dropwise, and the obtained product was repeatedly washed with deionized water and anhydrous ethanol for several times, and then the palladium ions in the polymer were removed with a 0.5 mol / L dilute hydrochloric acid solution until the supernatant was neutral and no palladium ions were detected by a color developer, and then dried in a vacuum drying oven for 12 h to obtain a palladium ion imprinted polymer Pd 2+ -IIP.

2. A palladium ion imprinted polymer Pd according to claim 1 2+ -A method for preparing IIP, characterized in that The amount of the KH-570 coupling agent used is 2.0 mL, the amount of sodium tetrachloropalladate Na2PdCl4 used is 0.05 g, the amount of magnetic microspheres Fe3O4 / SiO2 used is 0.40 g, the amount of the functional monomer DMAEMA used is 3 mmol, the reaction temperature is 40°C, and the reaction time is 8 h.

3. A palladium ion imprinted polymer Pd according to claim 1 2+ -A method for preparing IIP, characterized in that The preparation method of the magnetic microspheres Fe3O4 / SiO2 is as follows: the magnetic Fe3O4 is prepared by a coprecipitation method, 0.50 g of Fe3O4 and 1.0 g of hexadecyltrimethylammonium bromide (CTAB) are weighed in a beaker, 20 mL of deionized water and 200 mL of anhydrous ethanol are added, and the mixture is evenly dispersed by ultrasonication, and then the mixture is transferred to a three-necked flask and stirred for 30 min, and then 3 mL of tetraethyl orthosilicate (TEOS) is added, and 5 mL of ammonia water is added dropwise at 30°C, and the mixture is stirred for reaction for 24 h. After the reaction is completed, the separated sample is repeatedly washed with anhydrous ethanol and deionized water for several times, and then dried in a vacuum drying oven for 24 h. The product is placed in a muffle furnace and calcined at 550°C for 6 h. After cooling, the magnetic microspheres Fe3O4 / SiO2 are obtained.

4. A method for preparing a palladium ion imprinted polymer sensor, characterized in that: The preparation process includes the following steps: First, the glassy carbon electrode GCE with a diameter of 3 mm was pretreated. The surface of the glassy carbon electrode was polished with alumina powder with a particle size of 0.3 μm and 0.5 μm, respectively. It was repeatedly rinsed with anhydrous ethanol and deionized water, and ultrasonically washed in an ultrasonic cleaner for 3 min. The operation was repeated several times to remove the powder remaining on the surface of the glassy carbon electrode after polishing. It was blown dry with nitrogen to prevent oxidation, and activated with a 0.5 mol / L dilute sulfuric acid solution. Then 0.05 g of palladium ion-imprinted polymer Pd 2+ -IIP, anhydrous ethanol and Nafion perfluorinated resin solution were mixed and ultrasonicated for 30 min to form a uniform suspension, which was evenly dropped onto the surface of the activated glassy carbon electrode. After the ethanol evaporated at room temperature, a film was formed on the electrode surface, thus preparing a palladium ion imprinted polymer sensor.

Citation Information

Patent Citations

  • Preparation method of magnetic cadmium ion surface imprinted polymer

    CN103709342A

  • Novel method for detection of codeine based on ionic iridium complex electrochemiluminescence and molecular imprinting recognition

    CN105548151A

  • Electrochemical sensor for sensitively detecting heavy metal cadmium ions and preparation method of electrochemical sensor

    CN108318568A

  • Magnetic molecularly imprinted nano-composite-based electrochemical sensor, preparation method thereof and application of electrochemical sensor

    CN110632143A