Battery cell insulation sealing gasket based on polyurethane material and preparation method of battery cell insulation sealing gasket
Through the prepolymerization and polycondensation reaction of polyethylene glycol and isophorone diisocyanate, combined with the reinforcement of glass fiber, the problem of insufficient thermal stability of polyurethane materials is solved, and a battery cell insulation with high thermal stability and excellent mechanical properties is prepared. Sealing gaskets are suitable for replacing fluoroelastic materials and meet environmental protection requirements.
Patent Information
- Application Number
- CN202411138229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polyurethane materials are poor in thermal stability as battery-core insulating sealing gaskets. The long-term use temperature is usually below 100℃ and are prone to degradation at high temperatures. The fluoroelastic materials have high cost, poor low-temperature performance, difficult processing and great environmental impact. It is difficult to use in application scenarios with high environmental protection requirements.
Prepolymerization and polycondensation reaction were carried out by polyethylene glycol and isophorone diisocyanate to prepare an aqueous polyurethane emulsion, and polycondensation reaction was carried out at 45-55°C to improve the thermal stability of the polymer, and then with glass fibers, etc. The reinforcement material is composited and the battery-cell insulating sealing gasket is obtained through molding and curing.
Improve the thermal stability and mechanical properties of polyurethane materials. The thermal decomposition temperature reaches above 185℃, the glass transition temperature is below -16.6℃, and the mechanical properties are excellent. It can replace fluoroelastic rubber to prepare insulating sealing gaskets. It has green and environmentally friendly polymer materials. Features.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery core insulating gaskets, and particularly relates to a battery core insulating sealing gasket based on polyurethane material and a preparation method thereof. Background Art
[0002] Affected by the depletion of natural resources, there will be a serious shortage of natural energy such as oil, and the use of fuel vehicles will be limited; in comparison, the advantages of electric vehicles are becoming more and more obvious, and cylindrical batteries are increasingly widely used in electric vehicles. The top cover of the cylindrical battery cell is usually composed of a metal substrate, an insulating gasket, a pole, etc., which plays an insulating and sealing effect. Among them, the insulating gasket is a key component of battery performance and safety, and plays a variety of important roles in the battery cell: 1. It can prevent electrolyte leakage or external impurities from entering the battery, thereby maintaining the stability of the electrolyte and the normal operation of the battery; 2. Effectively isolate the metal contact between the positive and negative electrodes of the battery to prevent short circuits between the electrodes and ensure the safety and stability of the battery; 3. The insulating gasket usually has a certain degree of flexibility and elasticity, which can provide mechanical support and buffering between the internal components of the battery, help reduce the impact of vibration and shock on the battery cell, and improve the reliability and life of the battery.
[0003] Insulating gaskets must have appropriate mechanical flexibility and provide the required tightness. At present, most insulating gaskets on the market are made of insulating rubber or insulating silicone, and most of them are made of fluororubber as the base material. They not only have good elasticity and insulation properties, but also have good heat resistance. Fluororubber is made of fluorocarbon polymers and has excellent wear resistance, corrosion resistance and oxidation resistance. It is widely used in corrosive environments in the fields of automobiles, aerospace, petrochemicals, medicine, electronic components, etc. However, the high cost, poor low-temperature performance and difficult processing of such materials limit their use in certain specific applications. In particular, fluororubber contains fluorine elements, which may have a certain impact on the environment during its production and waste treatment. The degradation process may emit harmful substances, which is not suitable for application scenarios with high environmental protection requirements. In recent years, the European Union has revised the Battery Directive to require further improvement of environmental protection and resource efficiency. Therefore, with the further development of the new energy battery industry, it is necessary to find a fluorine-free polymer material to replace fluororubber in the production of insulating gaskets.
[0004] Polyurethane is a high-performance polymer material widely used in various industrial and consumer product fields. It has many advantages: 1. Polyurethane has high elasticity and flexibility, and can maintain good deformation recovery under a wide range of loads; 2. Polyurethane materials usually have excellent wear resistance and impact resistance, and are suitable for high wear environments; 3. Polyurethane has good resistance to many oils and chemicals, and is suitable for working environments that come into contact with grease and certain chemicals; 4. Polyurethane materials usually have good weather resistance and UV resistance, and are suitable for outdoor use; 5. Polyurethane can be manufactured through a variety of processes such as casting, spraying, foaming, extrusion, and injection molding, and has high design flexibility. However, this type of polymer material is highly correlated with the structure, and most polyurethane materials have poor thermal stability. The long-term use temperature is usually below 100°C, and they are easily degraded at high temperatures. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, provide a battery cell insulating sealing gasket based on polyurethane material and a preparation method thereof, and solve the technical problem in the prior art that polyurethane material as a battery cell insulating sealing gasket has poor thermal stability.
[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for preparing a battery cell insulating sealing gasket based on a polyurethane material, comprising the following steps: S1, prepolymerization: using polyethylene glycol and isophorone diisocyanate as raw materials, mixing them with a catalyst and an organic solvent, and then conducting a prepolymerization reaction to obtain a prepolymerization system; S2, polycondensation reaction: adding a chain extender and a capping agent to the prepolymerization system, and conducting a polycondensation reaction at 45 to 55° C. to obtain a reaction liquid; the reaction liquid is post-treated to obtain an aqueous polyurethane emulsion; S3, by mass percentage, 60 to 100% of the aqueous polyurethane emulsion and 0 to 40% of a reinforcing material are uniformly mixed to obtain a mixture, and the mixture is molded and cured to obtain a battery cell insulating sealing gasket.
[0007] In a second aspect, the present invention provides a polyurethane-based battery core insulating sealing gasket produced by the above method.
[0008] Compared with the prior art, the beneficial effects of the present invention include: The invention uses polyethylene glycol and isophorone diisocyanate as raw materials, and prepares an aqueous polyurethane emulsion through prepolymerization and polycondensation reaction, wherein the polycondensation reaction is carried out at 45-55 DEG C, the reaction temperature is relatively low, which is conducive to controlling the polymerization yield, and regulating the consistency of the physical and chemical properties of the polymer, thereby improving the thermal stability; the aqueous polyurethane emulsion is used as a matrix, and a certain proportion of reinforcing material is compounded to prepare an electric core insulating gasket product with excellent performance; the electric core insulating gasket of the invention has good thermal stability, a thermal decomposition temperature of more than 185 DEG C, a glass transition temperature of less than -16.6 DEG C, and excellent mechanical properties. DETAILED DESCRIPTION
[0009] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0010] Aiming at the problem that most polyurethane materials have poor thermal stability, long-term use temperature is usually below 100°C, and they are easy to degrade at high temperature, the present invention uses molecular structure design, first uses polyol PEG with higher thermal stability as raw material, introduces rigid segments in the polyurethane synthesis process, and improves the thermal stability of polyurethane by increasing the crosslinking density; then introduces a certain proportion of reinforcing materials through compounding, thereby improving the thermal stability and mechanical properties of polyurethane materials. The synthesized polyurethane composite material has excellent comprehensive performance and is a green and environmentally friendly polymer material that can replace fluororubber to prepare insulating sealing gaskets.
[0011] In a first aspect, the present invention provides a method for preparing a battery core insulating sealing gasket based on a polyurethane material, comprising the following steps: S1, prepolymerization: using polyethylene glycol and isophorone diisocyanate as raw materials, mixing with a catalyst and an organic solvent, and then performing a prepolymerization reaction to obtain a prepolymerization system; S2, polycondensation reaction: adding a chain extender and a capping agent to the prepolymerization system, carrying out a polycondensation reaction at 45-55° C. to obtain a reaction liquid; the reaction liquid is post-treated to obtain an aqueous polyurethane emulsion; S3, by mass percentage, 60-100% of aqueous polyurethane emulsion and 0-40% of reinforcing material are mixed uniformly to obtain a mixture, and the mixture is molded and cured to obtain a battery cell insulating sealing gasket.
[0012] Preferably, in step S1, the molar ratio of polyethylene glycol to isophorone diisocyanate is 1:(2-5); the polyethylene glycol is PEG-800.
[0013] Preferably, in step S1, the catalyst includes stannous isooctanoate; and the ratio of polyethylene glycol to the catalyst is 1 mmol: (10-50) mg.
[0014] Preferably, in step S1, the organic solvent includes acetone; and the ratio of polyethylene glycol to the organic solvent is 1 mmol: (1-15) mL.
[0015] Preferably, in step S1, the prepolymerization reaction is carried out under a protective atmosphere at 45 to 50° C. for 1.5 to 2.5 hours. The protective atmosphere is an inert gas. An increase in the prepolymerization temperature will have an adverse effect. A temperature above 50° C. will increase the instability of the molecular structure of the prepolymer, affecting the quality and performance of the final polymer product. Moreover, under high temperature conditions, the reaction rate is too fast, resulting in uneven polymerization reaction, making the molecular weight distribution of the polymer wider, and affecting the consistency and controllability of the physical and chemical properties of the product.
[0016] Preferably, in step S2, the chain extender and the end capping agent are first respectively prepared with acetone to form a chain extender solution and an end capping agent solution, and then added to the prepolymerization system; the chain extender includes one or both of 2,2-dihydroxymethylbutyric acid and 1,4-butanediol, and the end capping agent includes 1,4-butanediol.
[0017] More preferably, the molar ratio of 2,2-dimethylolbutyric acid, 1,4-butanediol and isophorone diisocyanate is 1:2:4.
[0018] Preferably, in step S2, the polycondensation reaction is carried out under a protective atmosphere; the polycondensation reaction time is 5.5 to 6.5 hours. In the polycondensation reaction of the present invention, the polymerization yield is controlled by appropriately lowering the reaction temperature, increasing the reaction time, and regulating the consistency of the physical and chemical properties of the polymer.
[0019] Preferably, in step S2, the post-treatment specifically comprises: adjusting the pH of the reaction solution to neutral with triethylamine, stirring for 5 to 10 minutes, adding water and stirring for emulsification, and then removing the organic solvent by rotary evaporation to obtain an aqueous polyurethane emulsion.
[0020] More preferably, the ratio of isophorone diisocyanate to water is (1-5) mmol:20 mL; the stirring emulsification is carried out at a speed of 600-800 rpm for 20-40 min; and the temperature of the rotary evaporation is 35-45° C. A too low stirring speed will affect the reaction efficiency.
[0021] Preferably, in step S3, by mass percentage, 60-99.9% of the aqueous polyurethane emulsion and 0.1-40% of the reinforcing material are uniformly mixed; more preferably, 60-95% of the aqueous polyurethane emulsion and 5-40% of the reinforcing material are mixed, and more preferably, 60-90% of the aqueous polyurethane emulsion and 10-40% of the reinforcing material are mixed.
[0022] Preferably, in step S3, the reinforcing material includes one or more of a fiber-reinforced material, a particle-reinforced material and a sheet-like reinforcing material.
[0023] Further preferably, the fiber reinforcement material includes one or more of glass fiber, carbon fiber, basalt fiber, aramid fiber, silicon carbide fiber and natural fiber; the particle reinforcement material includes one or more of carbon black, silicon dioxide particles, silicon nitride and silicon carbide; the sheet reinforcement material includes one or more of graphene, mica flakes and nanosheets. In order to improve the thermal stability of the material, the present invention preferably uses WPU-800 polyurethane material as the matrix material, and a certain proportion of glass fiber (GF) is compounded as the reinforcement material, preferably S-glass fiber or E-glass fiber as the reinforcement material.
[0024] During the mixing process, ensure that the glass fibers are evenly dispersed in the resin to avoid local strength inhomogeneities in the composite material.
[0025] Preferably, in step S3, the molding and curing is to add 1% of a photoinitiator to the mixture, mix well, and then inject it into a mold under high pressure. The mold is selected according to the shape actually required; and then it is cured by UV light in a UV oven for 5 minutes, so that the composite material obtains the required mechanical and thermal properties. After demolding, the cell insulation sealing gasket can be surface treated or subsequently processed to meet the specific requirements of the final application.
[0026] In a second aspect, the present invention provides a polyurethane-based battery core insulating sealing gasket produced by the above method.
[0027] The main mechanism of action and advantages of the present invention: (1) In order to retain the structural advantages of polyurethane materials to the greatest extent, in the preparation method of the present invention, a basic water-based polyurethane emulsion is first prepared, and isophorone diisocyanate (IPDI) and polyethylene glycol (PEG) are used as synthetic raw materials in the synthesis of the prepolymer; 2,2-dihydroxymethylbutyric acid (DMBA) is selected as a hydrophilic chain extender to improve the dispersibility of the polycondensation reaction product in the emulsion; 1,4-butanediol (BDO) with high reactivity is used as a chain extender and end-capping agent to increase the molecular weight of the polyurethane; finally, it is neutralized with triethylamine and then sheared and emulsified to obtain an emulsion.
[0028] The synthetic route of the aqueous polyurethane emulsion (WPU) in the present invention is:
[0029] (2) The materials used in the present invention are all common industrial materials with wide sources and low costs.
[0030] (3) In the actual application of polyurethane polymer materials, it is possible to consider adding reinforcing materials with high strength and high modulus such as fibers, particles or sheets to the base materials to improve their comprehensive properties such as mechanical properties, heat resistance, and corrosion resistance.
[0031] The present invention is further described in detail below through specific examples.
[0032] Example 1 S1, prepolymerization: 1mmol polyethylene glycol (PEG Mn=800) and 4mmol isophorone diisocyanate (IPDI) were added into a three-necked flask at a molar ratio of 1:4, 10mg catalyst stannous isooctanoate was added, and an anhydrous and oxygen-free reaction apparatus was built (inert gas argon was introduced); 10mL acetone was added to adjust the viscosity, and the prepolymerization reaction was carried out at 50°C for 2 h to obtain a prepolymerization system.
[0033] S2, polycondensation reaction: After the prepolymerization reaction is completed, 0.5 mol / L DMBA acetone solution and 1 mol / L BDO acetone solution are added to the prepolymerization system, respectively, with the molar ratio of DMBA, BDO and IPDI being 1:2:4, and the reaction is continued at 50°C for 6 hours under an argon atmosphere. After the reaction is completed, the heating is turned off, the reaction solution is cooled to room temperature, triethylamine is added to adjust the pH of the reaction solution to neutral, 20 mL of deionized water is added after stirring for 10 minutes, and emulsification is carried out at a high-speed shear stirring condition of 700 rpm for 30 minutes; the emulsified emulsion is taken out, and the acetone is removed by rotary evaporation at 40°C on a rotary evaporator to obtain a uniform and stable waterborne polyurethane emulsion.
[0034] S3, using the polyurethane emulsion obtained in step S2 as a matrix material, injecting it into a mold under high pressure, and demolding after molding and curing to obtain a battery cell insulating sealing gasket based on polyurethane material, which is recorded as WPU-800.
[0035] Example 2 The only difference from Example 1 is that in step S3, polyurethane WPU-800 is used as the matrix material, S-glass fiber (GF) is used as the reinforcing material, and by mass percentage, WPU-800 is 90% and GF is 10%. The other steps and conditions are the same as those in Example 1; the difference is that: S3: Using the polyurethane emulsion obtained in step S2 as the matrix material and S-glass fiber (GF) as the reinforcing material, the polyurethane emulsion and GF are mixed to obtain a mixture, and then the mixture is injected into a mold under high pressure. After molding and curing, the mixture is demolded to obtain a battery cell insulating sealing gasket based on polyurethane material, which is recorded as WPU-800-GF-10.
[0036] Example 3 The only difference from Example 2 is that 80% of the polyurethane emulsion and 20% of the GF are used, and the other steps and conditions are the same as those in Example 1. The obtained polyurethane-based battery cell insulating sealing gasket is recorded as WPU-800-GF-20.
[0037] Example 4 The only difference from Example 1 is that 70% of the polyurethane emulsion and 30% of the GF are used, and the other steps and conditions are the same as those in Example 1. The obtained battery cell insulating sealing gasket based on polyurethane material is recorded as WPU-800-GF-30.
[0038] Example 5 The only difference from Example 1 is that 60% of the polyurethane emulsion and 40% of the GF are used, and the other steps and conditions are the same as those in Example 1. The obtained battery cell insulating sealing gasket based on polyurethane material is recorded as WPU-800-GF-40.
[0039] Comparative Example 1 The only difference from Example 1 is that PEG 400 is used as polyethylene glycol, and the other steps and conditions are the same as those in Example 1. The obtained polyurethane material is recorded as WPU-400.
[0040] Comparative Example 2 The only difference from Example 1 is that PEG 2000 is used as polyethylene glycol, and the other steps and conditions are the same as those in Example 1. The obtained polyurethane material is recorded as WPU-2000.
[0041] The aqueous polyurethane emulsion prepared in the above Example 1 still maintains a uniform and stable emulsion state after being left to stand for 6 months.
[0042] The battery cell insulating sealing gaskets obtained in the above-mentioned embodiments and comparative examples were tested, and a control group was set up: the fluororubber sealing gaskets for cylindrical battery cells produced by Yukang Technology (Shanghai) Co., Ltd. were directly used as the control group; the thermal stability and crystallization kinetics of the polyurethane composite material were studied by thermal gravimetric analysis (TGA) and differential scanning calorimetry (DSC), and its thermal decomposition temperature and glass transition temperature were tested. The results are shown in Table 1 below.
[0043] Table 1 Thermal stability test of products with different polyurethane emulsion / GF mass ratios
[0044] As shown in Table 1, the WPU-800 prepared in Example 1 has a thermal decomposition temperature greater than 100°C, a glass transition temperature lower than -15°C, and good viscoelasticity, and can be used as a sealing gasket; while the polyurethane material WPU-400 obtained in Comparative Example 1 is in a brittle wafer state at room temperature, and the polyurethane material WPU-2000 obtained in Comparative Example 2 is in a gel state at room temperature and does not have basic mechanical properties; TG and DSC test results also show that PEG of different molecular weights has a great influence on the thermal stability of the synthesized WPU. Only the WPU-800 material synthesized by PEG with Mn=800 and IPDI has a comprehensive thermal stability close to that of fluororubber, and has the potential to be cured and molded into an insulating rubber gasket, while the polyurethane materials obtained in Comparative Examples 1 and 2 cannot be used as sealing gaskets.
[0045] In Examples 2-5 of the present invention, 10% to 40% of glass fiber is introduced as a reinforcing material by composite blending into a polyurethane emulsion synthesized from PEG and isophorone diisocyanate (IPDI). It is found that the introduction of glass fiber can increase the thermal decomposition temperature of the material to a certain extent, and improve its thermal stability under high-temperature working environment; although the glass transition temperature is increased, it can still meet the basic application requirement of -15°C.
[0046] The products obtained in Examples 1-5 were tested for various mechanical properties, specifically: ISO 178 flexural property test (flexural modulus and maximum strength) and ISO 527 tensile property test (tensile modulus, yield stress, yield elongation, breaking stress, breaking elongation and tensile strength). The results are shown in Table 2 below.
[0047] Table 2 Mechanical properties test of products with different polyurethane emulsion / GF mass ratios
[0048] As shown in Table 2, by conducting relevant mechanical property tests on the synthesized polyurethane-based battery cell insulation sealing gaskets, it is found that the introduction of glass fiber can not only increase the thermal decomposition temperature of the material to a certain extent, but also effectively improve the mechanical properties such as yield stress, fracture stress, and tensile strength, and improve the overall performance of the composite material. Among them, the battery cell insulation sealing gasket obtained by compounding 20wt% of glass fiber as a reinforcing material has the best comprehensive performance and is expected to become a new environmentally friendly polymer material to replace fluororubber to prepare insulation sealing gaskets.
[0049] Comparative Example 3 The only difference from Example 1 is that the prepolymerization and polymerization temperatures are changed to 70° C., and the other steps and conditions are the same as those of Example 1. The polyurethane emulsions obtained in Example 1 and Comparative Example 3 were tested, and the results are shown in Table 3 below.
[0050] Table 3 Comparison of polyurethane emulsions obtained in Example 1 and Comparative Example 3
[0051] From the results in Table 3, it is found that when the prepolymerization and polymerization temperatures are increased to 70°C (higher than 50°C), the obtained emulsion is milky white, with a solid content of 19.18%, a viscosity of 63.27mpa / s, and a polymer state of gel. This indicates that temperatures above 50°C increase the instability of the molecular structure of the prepolymer, affecting the quality and performance of the final polymer product. Moreover, under high temperature conditions, the reaction rate is too fast, resulting in uneven polymerization, making the molecular weight distribution of the polymer wider, affecting the consistency and controllability of the physical and chemical properties of the product, and unable to prepare an insulating gasket product with excellent performance.
[0052] In summary, the present invention provides a battery cell insulating sealing gasket based on polyurethane material and a preparation method thereof, wherein a polyurethane emulsion is prepared by prepolymerization and polycondensation reaction, and a composite polymer material with excellent comprehensive performance is synthesized using polyurethane as a base material and glass fiber as a reinforcing material, which can be processed and extruded into an insulating sealing gasket, wherein the composite ratio can be specifically regulated according to specific application requirements and desired performance, such as 60-100% of polyurethane emulsion and 0-40% of reinforcing material, which can be specifically regulated according to specific application requirements and desired performance; by selecting monomers of polyurethane polymer materials and controlling synthesis conditions, the present invention adopts polyethylene glycol with Mn=800 as a raw material and glass fiber as a reinforcing material, controls prepolymerization and polycondensation temperature, reaction time and other conditions, and provides a new polyurethane polymer material with excellent performance that can be used in various aspects such as the automotive industry, especially as a battery cell insulating sealing gasket.
[0053] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a battery core insulating sealing gasket based on polyurethane material, characterized in that: The following steps are involved: S1, prepolymerization: using polyethylene glycol and isophorone diisocyanate as raw materials, mixing with a catalyst and an organic solvent, and then performing a prepolymerization reaction to obtain a prepolymerization system; S2, polycondensation reaction: adding a chain extender and a capping agent to the prepolymerization system, performing a polycondensation reaction at 45-55° C. to obtain a reaction liquid; the reaction liquid is post-treated to obtain an aqueous polyurethane emulsion; S3, by mass percentage, 60-100% of aqueous polyurethane emulsion and 0-40% of reinforcing material are mixed uniformly to obtain a mixture, and the mixture is molded and cured to obtain a battery cell insulating sealing gasket.
2. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S1, the molar ratio of the polyethylene glycol to the isophorone diisocyanate is 1:(2-5); the polyethylene glycol is PEG-800.
3. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S1, the catalyst includes stannous isooctanoate; the ratio of the polyethylene glycol to the catalyst is 1 mmol: (10-50) mg; The organic solvent includes acetone.
4. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S1, the prepolymerization reaction is carried out under a protective atmosphere at 45-50° C. for 1.5-2.5 hours.
5. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S2, the chain extender includes one or both of 2,2-dihydroxymethylbutyric acid and 1,4-butanediol, and the end-capping agent includes 1,4-butanediol.
6. The method for preparing a polyurethane-based battery core insulating sealing gasket according to claim 5, characterized in that: The molar ratio of the 2,2-dihydroxymethylbutyric acid, the 1,4-butanediol and the isophorone diisocyanate is 1:2:
4.
7. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S2, the polycondensation reaction is carried out under a protective atmosphere; the polycondensation reaction time is 5.5 to 6.5 hours.
8. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S2, the post-treatment specifically includes: adjusting the pH of the reaction solution to neutral with triethylamine, stirring for 5 to 10 minutes, adding water and stirring for emulsification, and then removing the organic solvent by rotary evaporation to obtain an aqueous polyurethane emulsion; The ratio of the isophorone diisocyanate to the water is (1-5) mmol:20 mL.
9. The method for preparing a battery core insulating sealing gasket based on polyurethane material according to claim 1, characterized in that: In step S3, 60 to 99.9% of the aqueous polyurethane emulsion and 0.1 to 40% of the reinforcing material are mixed uniformly by mass percentage; the reinforcing material includes one or more of a fiber-reinforced material, a particle-reinforced material and a sheet-like reinforcing material.
10. A battery core insulating sealing gasket based on polyurethane material prepared by the preparation method according to any one of claims 1 to 9.