Bio-based polyurethane elastomer as well as preparation method and degradation method thereof
By using bio-based raw materials to prepare non-crystalline polyester glycol and highly regular isocyanate, the degree of microphase separation and physical crosslinking density of polyurethane is improved, and the problem of difficult degradation of polyurethane materials is solved, and the combination of rapid degradation and good mechanical properties is achieved is achieved. .
Patent Information
- Application Number
- CN202411047541.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Existing polyurethane materials are difficult to degrade, resulting in environmental pollution, and their structural characteristics affect the degradation efficiency.
Use bio-based raw materials to prepare non-crystalline soft segments and highly regular hard segments to improve the micro-phase separation degree and physical cross-linking density of polyurethane, design bio-based polyester glycol and isocyanate with straight chain structures, reduce the content and crystallization of hard segments Area, the degradability and mechanical properties of the reinforced material.
The rapid degradation and good mechanical properties of polyurethane materials are achieved, and the degradation rate can reach 70-88% within 20 days, while ensuring the overall performance of the material.
Smart Images

Figure CN118930800A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and more particularly to a bio-based polyurethane elastomer and a preparation method and a degradation method thereof. Background Art
[0002] Polyurethane is a block copolymer, which is composed of a flexible soft segment and a rigid hard segment. The soft segment is generally a hydroxyl-terminated polyester or polyether diol with a molecular weight of 500-5000 g / mol, and the hard segment is a diisocyanate and a low molecular weight chain extender. Due to the huge difference in solubility parameters between the soft segment and the hard segment, under the action of thermodynamics, they spontaneously aggregate into hard segment aggregates with high hard segment content and soft segment aggregates with high soft segment content. Due to the sea island structure produced by microphase separation, the hard segment aggregates of polyurethane have a self-reinforcement effect on the material, making polyurethane have excellent strength, resilience, wear resistance, oil resistance and other excellent properties. Therefore, polyurethane materials can be widely used in shoe materials, conveyor belts, biomedical, sealing products and other fields.
[0003] As petrochemical raw materials are gradually depleted and people pursue a low-carbon and environmentally friendly life, people have begun to call for the preparation of polymer products with bio-based raw materials. Therefore, the use of bio-based raw materials to prepare rapidly degradable bio-based polyurethane elastomers is of great significance to the sustainable development of the polyurethane industry. However, most of the polyurethane materials currently developed are difficult to degrade and take hundreds of years to completely decompose in the environment. Therefore, a large amount of discarded polyurethane materials every year cause serious pollution to the environment.
[0004] The degradation of polyurethane usually includes different methods such as soil burial degradation, composting degradation, chemical recycling degradation, and enzyme degradation. Among them, enzyme degradation is the decomposition reaction of water and ester groups and carbamate groups catalyzed by enzymes. It is a degradation method with low energy consumption and fast degradation rate. In the process of enzyme degradation, the difficulty of polyurethane degradation is related to the widely distributed crystalline regions in the molecular structure, the degree of phase separation, and the soft segment chain structure: on the one hand, the hydrophobic crystalline structure hinders the interaction between water and easily degradable ester groups, affecting the degradation efficiency; on the other hand, when the degree of phase separation of polyurethane is small, the soft segment is more easily dissolved in the hard segment aggregate, and the hard segment that is difficult to degrade hinders the interaction between the easily degradable soft segment and degradation factors such as water and enzymes, resulting in a decrease in the degradation rate of polyurethane; on the other hand, the shielding effect produced by the side group structure of the soft segment will hinder the action of ester groups and water, and play a decelerating role in the reaction of ester groups decomposing into carboxyl groups and hydroxyl groups.
[0005] It can be seen that developing a polyurethane material with excellent comprehensive performance and rapid degradation is an urgent problem to be solved. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a bio-based polyurethane elastomer and a preparation method thereof. The bio-based polyurethane elastomer provided by the present invention not only has good comprehensive performance, but also has excellent degradability.
[0007] Firstly, one of the objects of the present invention is to provide a bio-based polyurethane elastomer.
[0008] Specifically, the bio-based polyurethane elastomer includes a soft segment and a hard segment, and the mass ratio of the soft segment to the hard segment is 74-88:12-26; preferably 75-85:15-25; wherein the soft segment is a non-crystalline bio-based polyester diol structural unit; and the hard segment is a structural unit composed of isocyanate and a bio-based chain extender.
[0009] The present invention reduces the content of crystalline regions in polyurethane by preparing completely non-crystallized soft segments, and uses highly regular isocyanate and a chain extender with a regular structure to improve the microphase separation degree of polyurethane. The obtained polyurethane elastomer not only has the performance of being rapidly degradable, but also has good comprehensive performance.
[0010] Furthermore, in the bio-based polyurethane elastomer, the bio-based polyester diol structural unit is a linear molecular chain segment structure with double hydroxyl end-capping, and the molecular weight is 500-2000 g / mol, preferably 1000-1500 g / mol. At this time, the hard segment of the polyurethane has a better packing density, the reinforcing effect of the hard segment aggregate is better, and for the non-crystallized soft segment, it is more conducive to the improvement of mechanical properties.
[0011] Further, in the bio-based polyurethane elastomer, the bio-based polyester diol structural unit contains no or a small amount of side groups.
[0012] Furthermore, in the bio-based polyurethane elastomer, the content of branched small molecules in the bio-based polyester diol structural unit is less than or equal to 20wt%.
[0013] Furthermore, in the bio-based polyurethane elastomer, the non-crystallized bio-based polyester diol is obtained by polycondensation of at least two bio-based raw materials, and the molar ratio of carboxyl groups to hydroxyl groups in the bio-based raw materials participating in the polycondensation reaction is 1:1.05 to 2, preferably 1:1.12 to 1.8.
[0014] The present invention increases the randomness of the bio-based polyester diol molecular chain by random polycondensation of multiple bio-based raw materials to reduce the crystallization tendency of the soft segment; at the same time, the bio-based raw materials used contain no or a small amount of side groups, and the obtained polyester diol is in a completely non-crystalline state with a mainly straight-chain structure.
[0015] Furthermore, the bio-based raw material is selected from dimethyl oxalate, dimethyl malonate, succinic acid, glutaric acid, adipic acid, sebacic acid, diglycolic acid, terephthalic acid, methyl itaconate, tridecanedioic acid, tetradecanedioic acid, α-hydroxypropionic acid, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, butanediol, 2,3-butanediol, pentanediol, and diethylene glycol.
[0016] Furthermore, the isocyanate is selected from at least one of p-phenylene diisocyanate, m-xylylene diisocyanate, hexamethylene diisocyanate and 1,5-pentamethylene diisocyanate.
[0017] Furthermore, the bio-based chain extender is selected from at least one of 1,6-hexanediol, 1,5-pentanediol, 1,4-butanediol, 1,3-propylene glycol, and ethylene glycol.
[0018] Secondly, the second object of the present invention is to provide a method for preparing the bio-based polyurethane elastomer of one of the objects of the present invention, the preparation method comprising the following steps:
[0019] S1. Add the bio-based raw material into a reaction vessel, raise the temperature to 150-200° C., carry out esterification reaction for 2-6 hours, add a catalyst, reduce the pressure to -0.1-0.08 MPa, and terminate the reaction when the hydroxyl value reaches 50-230 mg KOH / g to obtain a bio-based polyester diol;
[0020] S2. Heat the bio-based polyester diol to 45-80° C., add isocyanate, and react for 2-3 hours; add a chain extender, stir evenly, degas, pour into a mold, hot-press mold at 100-160° C., and mature at 80-130° C. for 12-96 hours to obtain the polyurethane elastomer.
[0021] Preferably, in step S1, the catalyst needs to be dissolved in a solvent to prepare a solution before adding it to the reaction system, wherein the solvent is selected from at least one of ethylene glycol, 1,2-propylene glycol, toluene, and xylene. The mass concentration of the catalyst is 5 to 100 g / L; the amount of the catalyst solution is 0.1 to 3% of the total amount of the bio-based diacid and diol.
[0022] More specifically, the preparation method comprises the following steps:
[0023] S1. Add the bio-based raw material into a reaction vessel, replace the air twice with nitrogen at room temperature, raise the temperature to 150-200° C., carry out esterification reaction for 2-6 hours, add the catalyst solution, reduce the pressure to a vacuum degree of about -0.1-0.08 MPa, and continue until the acid value decreases to below 1 mg KOH / g and the hydroxyl value reaches 56-224 mg KOH / g to terminate the reaction and obtain bio-based polyester diol;
[0024] S2. Heat the bio-based polyester diol to 45-80°C, add isocyanate, and react for 2-3 hours; add chain extender, quickly stir, decompress and degas, pour into a mold, and send it to a hot press at 100-160°C for hot pressing. After 5-10 minutes, take out the sample from the mold, send the sample to an oven at 80-130°C for aging for 12-96 hours to obtain the polyurethane elastomer.
[0025] Again, the third object of the present invention is to provide a method for degrading a bio-based polyurethane elastomer according to one of the objects of the present invention, the degradation method comprising the following steps:
[0026] The bio-based polyurethane elastomer sample is crushed, put into a potassium dihydrogen phosphate / dipotassium hydrogen phosphate solution to prepare a mixed solution, and a degradation enzyme is added to degrade it to obtain a degradation solution.
[0027] Preferably, the pH of the potassium dihydrogen phosphate / dipotassium hydrogen phosphate solution is 6.9-7.4.
[0028] Preferably, the degradation temperature is 30-60°C.
[0029] Preferably, the mass concentration of the polyurethane elastomer in the mixed solution is 50 to 200 g / L.
[0030] Preferably, the amount of the degrading enzyme used is 0.5 to 2 times the mass of the polyurethane elastomer.
[0031] Preferably, the degrading enzyme is selected from Novozymes non-immobilized lipase A, Novozymes non-immobilized lipase B, and porcine pancreatic lipase.
[0032] Preferably, the degradation time is 2 to 40 days.
[0033] Compared with the prior art, the beneficial effects of the present invention are:
[0034] 1. The present invention improves the degradation rate of the bio-based polyurethane elastomer by reducing the hard segment content of the material and the proportion of the difficult-to-degrade urethane bonds; at the same time, in order to compensate for the decrease in the strength of the polyurethane caused by the reduction in the hard segment content and the lack of crystallization of the soft segment, a soft segment with a lower molecular weight and a hard segment with high regularity are used to improve the microphase separation degree of the material, better improve the physical crosslinking density of the material, and supplement its strength, so that the polyurethane elastomer has better comprehensive performance and also ensures rapid degradation performance.
[0035] 2. The present invention improves the phase separation degree of the polyurethane material, reduces the compatibility of the soft segment and the hard segment, and increases the degradation rate of the polyurethane by using highly regular diisocyanates and chain extenders.
[0036] 3. The bio-based polyester diol and chain extender of the present invention are both prepared from bio-based raw materials, and the bio-based content in the polyurethane elastomer is above 83%.
[0037] 4. The present invention designs the soft segment and hard segment structures of the polyurethane elastomer separately, selects non-crystalline, linear-structured bio-based polyester diols, highly regular-structured isocyanates and chain extenders, and obtains a rapidly degradable bio-based polyurethane elastomer. Under the catalysis of enzymes, the degradation rate of the bio-based polyurethane elastomer can be as high as 70-88% within 20 days. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a DSC test chart of the bio-based polyester diol prepared in Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0040] In the following examples and comparative examples, the raw materials are all derived from commercially available products.
[0041] In the test methods of the following embodiments, the corresponding test methods are as follows:
[0042] DSC test: In a nitrogen atmosphere, the sample was cooled from room temperature to -80°C at a rate of 10°C / min, kept at this temperature for 5 minutes, and then heated to 100°C at a rate of 10°C / min. The glass transition temperature (T g ), melting temperature, crystallization temperature and other information.
[0043] Mechanical properties test: The test was conducted according to the ASTM-D412 method, and the samples were cut into dumbbell-shaped specimens that met the test standards for testing.
[0044] Example 1
[0045] The following is used to illustrate the preparation of bio-based polyester diol. The specific preparation process is as follows:
[0046] The bio-based raw materials of succinic acid, sebacic acid, 1,3-propylene glycol and 1,2-propylene glycol were weighed in a molar ratio of 7:3:1.3:11.7 (acid alcohol ratio 1:1.3) with a total mass of 350g and put into a 500ml reaction container. After replacing the nitrogen, the reaction temperature was raised to 170℃, the reaction was carried out for 4h, and 4g of catalyst (tetrabutyl titanate-toluene, the concentration of the catalyst solution was 10wt%) was added, and the mass of the catalyst was 0.3% of the mass of the reactants. After stirring and mixing, the pressure was uniformly reduced to a vacuum degree of -0.09MPa within 1h. After that, the reaction was continued for 20min, and the reaction was stopped when the hydroxyl value reached 75mg KOH / g, and a bio-based polyester diol with a molecular weight of 1500g / mol was obtained.
[0047] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0048] The bio-based polyester diol prepared above was heated to 80°C, hexamethylene diisocyanate was added (the molar ratio of bio-based polyester diol and hexamethylene diisocyanate was 1:1.5), and the reaction was continued for 2.5 hours; the chain extender 1,4-butanediol (the molar ratio of bio-based polyester diol and 1,4-butanediol was 1:0.5) (the mass ratio of the soft segment to the hard segment was 83:17), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to an oven at 80°C for aging for 48 hours. It can be used for testing and practical applications after being stored at room temperature for 2 weeks.
[0049] The biobased content of the formula sample is 84.0%, and its mechanical properties are shown in Table 1.
[0050] Example 2
[0051] The following is used to illustrate the preparation of bio-based polyester diol. The specific preparation process is as follows:
[0052] Weigh 350g of bio-based raw materials in a molar ratio of 1:1:2.5 (acid-alcohol ratio 1:1.25) of bio-based glutaric acid, diglycolic acid, and pentanediol, and put them into a 500ml reaction container. After replacing nitrogen, increase the reaction temperature to 200℃, react for 4h, add 6g of catalyst (diethanol antimony-toluene, the concentration of the catalyst solution is 80g / l), and the catalyst mass is 0.15% of the total reactants. After stirring and mixing, reduce the pressure uniformly to a vacuum degree of -0.09MPa within 1h. After that, continue the reaction for 15min, and stop the reaction when the hydroxyl value reaches 112mg KOH / g to obtain a bio-based polyester diol with a molecular weight of 1000g / mol.
[0053] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0054] The bio-based polyester diol prepared above was heated to 80°C, p-phenylene diisocyanate was added (the molar ratio of bio-based polyester diol to p-phenylene diisocyanate was 1:1.5), and the reaction was continued for 2 hours; the chain extender 1,3-propylene glycol (the molar ratio of bio-based polyester diol to 1,3-propylene glycol was 1:0.5) (the mass ratio of the soft segment to the hard segment was 77:23), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 100°C oven for aging for 48 hours. It can be used for testing and practical applications after being stored at room temperature for 2 weeks.
[0055] The biobased content of this formula sample is 83.2%, and its mechanical properties are shown in Table 1.
[0056] Example 3
[0057] The following is used to illustrate the preparation of bio-based polyester diol. The specific preparation process is as follows:
[0058] Weigh 350g of bio-based raw materials in a molar ratio of 1:0.91:0.39 (acid-alcohol ratio 1:1.3) of bio-based glutaric acid, 1,3-propylene glycol, and 1,2-propylene glycol, and put them into a 500ml reaction container. After replacing nitrogen, raise the reaction temperature to 200℃, react for 4h, add 3.5g of catalyst (diethanol antimony-1,2-propylene glycol, mass concentration is 10%) solution, and the catalyst mass is 0.15% of the total reactants. After stirring and mixing, reduce the pressure uniformly to a vacuum degree of -0.09MPa within 1h. After that, continue the reaction for 30min, stop the reaction when the hydroxyl value reaches 75mg KOH / g, and obtain a bio-based polyester diol with a molecular weight of 1500g / mol.
[0059] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0060] The bio-based polyester diol prepared above was heated to 60°C, 1,5-pentamethylene diisocyanate was added (the molar ratio of bio-based polyester diol and 1,5-pentamethylene diisocyanate was 1:1.75), and the reaction was continued for 1.5 hours; the chain extender 1,4-butanediol (the molar ratio of bio-based polyester diol and 1,4-butanediol was 1:0.75) (the mass ratio of the soft segment to the hard segment was 81:19), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 130°C oven for aging for 48 hours. It can be used for testing and practical applications after being stored at room temperature for 2 weeks.
[0061] The bio-based content of the formula sample is 100%, and its mechanical properties are shown in Table 1.
[0062] Figure 1 This is the DSC test graph of the above Examples 1 to 3. It can be seen from the figure that the bio-based polyester diol prepared in Examples 1 to 3 has a glass transition process in the range of -80 to 100°C, but there is no obvious melting or crystallization peak, which indicates that the bio-based polyester diol prepared in Examples 1 to 3 is a completely non-crystalline polymer.
[0063] Example 4
[0064] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0065] The bio-based polyester diol in Example 1 was heated to 60°C, hexamethylene diisocyanate was added (the molar ratio of bio-based polyester diol to hexamethylene diisocyanate was 1:1.75), and the reaction was continued for 1.5 hours; the chain extender ethylene glycol was added (the molar ratio of bio-based polyester diol to ethylene glycol was 1:0.75) (the mass ratio of the soft segment to the hard segment was 81:19), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 110°C oven for aging for 48 hours. It can be used for testing and practical applications after being left at room temperature for 2 weeks.
[0066] The biobased content of this formula sample is 83.3%, and its mechanical properties are shown in Table 1.
[0067] Example 5
[0068] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0069] The bio-based polyester diol in Example 1 was heated to 60°C, 1,5-pentamethylene diisocyanate was added (the molar ratio of bio-based polyester diol and 1,5-pentamethylene diisocyanate was 1:1.5), and the reaction was continued for 1.5 hours; the chain extender 1,5-pentanediol (the molar ratio of bio-based polyester diol and 1,5-pentanediol was 1:0.5) (the mass ratio of the soft segment to the hard segment was 84:16), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 110°C oven for aging for 48 hours. It can be used for testing and practical applications after being left at room temperature for 2 weeks.
[0070] The bio-based content of the formula sample is 100%, and its mechanical properties are shown in Table 1.
[0071] Example 6
[0072] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0073] The bio-based polyester diol in Example 1 was heated to 60°C, 1,5-pentamethylene diisocyanate was added (the molar ratio of bio-based polyester diol and 1,5-pentamethylene diisocyanate was 1:1.5), and the reaction was continued for 1.5 hours; the chain extender 1,6-hexanediol (the molar ratio of bio-based polyester diol and 1,6-hexanediol was 1:0.5) (the mass ratio of the soft segment to the hard segment was 83:17), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 110°C oven for aging for 48 hours. It can be used for testing and practical applications after being left at room temperature for 2 weeks.
[0074] The bio-based content of the formula sample is 100%, and its mechanical properties are shown in Table 1.
[0075] Comparative Example 1
[0076] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0077] Poly(hexanediol adipate) (molecular weight 1500g / mol, crystalline) was heated to 80℃, hexamethylene diisocyanate (molar ratio of poly(hexanediol adipate) and hexamethylene diisocyanate was 1:1.5), and the reaction was continued for 2.5h; chain extender 1,4-butanediol (molar ratio of poly(hexanediol adipate) and 1,4-butanediol was 1:0.5) (mass ratio of soft segment to hard segment was 84:16), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and hot-pressed in a 110℃ hot press. The sample was removed from the mold after 5min. The sample was placed in an oven at 80℃ for 48h. After being stored at room temperature for 2 weeks, it can be used for testing and practical applications. The mechanical properties are shown in Table 1.
[0078] Comparative Example 2
[0079] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0080] The bio-based polyester diol prepared in Example 1 was heated to 80°C, dicyclohexylmethane diisocyanate was added (the molar ratio of bio-based polyester diol and dicyclohexylmethane diisocyanate was 1:1.16), and the reaction was continued for 2.5 hours; the chain extender 1,4-butanediol (the molar ratio of bio-based polyester diol and bio-based 1,4-butanediol was 1:0.16) (the mass ratio of the soft segment to the hard segment was 83:17) was added, and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a 130°C hot press for hot pressing. The sample was taken out of the mold after 20 minutes. The sample was sent to a 100°C oven for aging for 48 hours. After being parked at room temperature for 2 weeks, it can be used for testing and practical applications. The mechanical properties are shown in Table 1.
[0081] Comparative Example 3
[0082] The following is used to illustrate the preparation of bio-based polyester diol. The specific preparation process is as follows:
[0083] Weigh 350g of bio-based raw materials in a molar ratio of 1:1.3 (acid-alcohol ratio 1:1.3) of bio-based glutaric acid and 1,2-propylene glycol, and put them into a 500ml reaction container. After replacing nitrogen, the reaction temperature was raised to 200℃, the reaction was carried out for 4h, and 7g of catalyst (diethanol antimony-1,2-propylene glycol, mass concentration is 100g / L) solution was added, and the mass of the catalyst was 0.15% of the reactants. After stirring and mixing, the pressure was uniformly reduced to a vacuum degree of -0.09MPa within 1h. After that, the reaction was continued for 30min, and the reaction was stopped when the hydroxyl value reached 75mg KOH / g, and a bio-based polyester diol with a molecular weight of 1500g / mol was obtained.
[0084] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0085] The bio-based polyester diol prepared above was heated to 60°C, 1,5-pentamethylene diisocyanate was added (the molar ratio of bio-based polyester diol and 1,5-pentamethylene diisocyanate was 1:1.75), and the reaction was continued for 1.5 hours; the chain extender 1,4-butanediol (the molar ratio of bio-based polyester diol and 1,4-butanediol was 1:0.75) (the mass ratio of the soft segment to the hard segment was 81:19), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to a 130°C oven for aging for 48 hours. After being stored at room temperature for 2 weeks, it can be used for testing and practical applications. The mechanical properties are shown in Table 1.
[0086] Comparative Example 4
[0087] eTPU-95a (purchased from Shenzhen Guanghua Weiye Co., Ltd.) is a commercial, biodegradable bio-based polyurethane elastomer.
[0088] The molding method of the sample is as follows: the pellets of eTPU-95a are placed in a 2 cm mold, preheated in a hot press at 160°C for 10 minutes, then hot pressed for 10 minutes, cooled at room temperature for 10 minutes and taken out, and placed for 2 weeks for testing and practical application. The mechanical properties are detailed in Table 1.
[0089] Comparative Example 5
[0090] The following is used to illustrate the preparation of bio-based polyurethane elastomer. The specific preparation process is as follows:
[0091] The bio-based polyester diol in Example 1 was heated to 80°C, hexamethylene diisocyanate was added (the molar ratio of bio-based polyester diol to hexamethylene diisocyanate was 1:2.75), and the reaction was continued for 2.5 hours; the chain extender 1,4-butanediol (the molar ratio of bio-based polyester diol to 1,4-butanediol was 1:1.75) (the mass ratio of the soft segment to the hard segment was 70:30), and the mixture was quickly stirred, degassed under reduced pressure, poured into a mold, and sent to a hot press for hot pressing. The sample was taken out of the mold after 5 minutes. The sample was sent to an oven at 80°C for aging for 48 hours. It can be used for testing and practical applications after being left at room temperature for 2 weeks.
[0092] The biobased content of this formula sample is 77.9%, and its mechanical properties are shown in Table 1.
[0093] The polyurethane materials prepared in the above Examples 1 to 6 and the polyurethane materials in Comparative Examples 1 to 5 were subjected to a degradation performance test. The specific degradation performance test steps are as follows:
[0094] First, crush the sample into pieces with a volume less than 4 mm. 3 Cubes, then mix the crushed sample with potassium dihydrogen phosphate / dipotassium hydrogen phosphate solution at 37°C, pH=7.4, prepare the sample into a mixed solution with a concentration of 50g / L, and then add Novozymes non-immobilized lipase CLAB (enzyme activity is 5000LU / g, the ratio of enzyme solution mass to sample mass is 1:1), stir and mix, and continue to degrade for 20 days. After the degradation is completed, the degradation solution is centrifuged and the lower layer residue of the centrifuged solution is collected. The residue is dried under reduced pressure in a freeze dryer at 0°C. Finally, weigh the residue and calculate the mass loss rate during the degradation process, which is the degradation rate. The specific degradation performance test results are shown in Table 1.
[0095] The mechanical property test and degradation test results of the bio-based polyurethane elastomers of Examples 1 to 4 and the polyurethane elastomers of Comparative Examples 1 to 4 are shown in Table 1, and are specifically as follows:
[0096]
[0097] It can be seen from the data in Table 1 that the polyurethane materials prepared in Examples 1 to 6 have good mechanical properties, can meet the application requirements, and have good degradation properties.
[0098] Comparative Example 1 uses crystalline poly(hexanediol adipate) as the soft segment, and the degradation rate after 20 days is significantly reduced.
[0099] From the comparison between Example 1 and Comparative Example 2, it can be seen that Example 1 selected hexamethylene diisocyanate (HDI) and 1,4-butanediol (BDO) with good regularity as the hard segment of the polyurethane, while Comparative Example 2 selected dicyclohexylmethane diisocyanate (HMDI) with poor regularity as the hard segment of the polyurethane. The irregular hard segment chain reduces the microphase separation degree of the polyurethane, which not only leads to poor mechanical properties, but also greatly reduces its degradation rate. Compared with the polyurethane in Example 1, the tensile strength and degradation rate of the polyurethane in Comparative Example 2 are reduced by 95.2% and 87.5%, respectively.
[0100] By comparing Example 3 (the mass ratio of side group small molecules to bio-based polyester diol is 17.9%) and Comparative Example 3 (the mass ratio of side group small molecules to bio-based polyester diol is 42.8%), it can be seen that the content of side groups in the soft segment of Comparative Example 3 is higher, and due to the shielding effect of the side groups, the polyurethane is difficult to degrade. Compared with Example 3, the 20-day degradation rate of the polyurethane in Comparative Example 3 is reduced by 52.6%.
[0101] It can be seen from Comparative Example 4 that when commercial degradable polyurethane is used, the bio-based polyurethane provided by Examples 1 to 6 has obvious advantages in degradation performance within 20 days.
[0102] It can be seen from the comparison between Example 1 and Comparative Example 5 that when the hard segment content in the polyurethane is too high, when the hard segment content in Comparative Example 5 reaches 30%, the degradation rate of the material will be greatly reduced.
[0103] In summary, the bio-based polyester diol provided by the present invention, which is mainly straight-chain, has no side groups or has a low side group content, is used as the soft segment, and is combined with a regular hard segment chain, which not only helps to improve the mechanical properties of the polyurethane, but also greatly improves the degradation performance of the material.
[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A bio-based polyurethane elastomer, comprising a soft segment and a hard segment, wherein the soft segment is a non-crystalline bio-based polyester diol structural unit, the hard segment is a structural unit composed of isocyanate and a bio-based chain extender, and the mass ratio of the soft segment to the hard segment is 74-88:12-26.
2. The bio-based polyurethane elastomer according to claim 1, characterized in that The bio-based polyester diol structural unit is a linear molecular segment structure double-terminated by hydroxyl groups, and has a molecular weight of 500 to 2000 g / mol.
3. The bio-based polyurethane elastomer according to claim 1, characterized in that The bio-based polyester diol structural unit contains no or a small amount of side groups; and / or the content of branched small molecules in the bio-based polyester diol structural unit is less than or equal to 20wt%.
4. The bio-based polyurethane elastomer according to claim 1, characterized in that The bio-based polyester diol is obtained by polycondensation of at least two bio-based raw materials, and the molar ratio of carboxyl groups to hydroxyl groups in the bio-based raw materials participating in the polycondensation reaction is 1:1.05-2.
5. The bio-based polyurethane elastomer according to claim 4, characterized in that The bio-based raw material is selected from dimethyl oxalate, dimethyl malonate, succinic acid, glutaric acid, adipic acid, sebacic acid, diglycolic acid, terephthalic acid, methyl itaconate, tridecanedioic acid, tetradecanedioic acid, α-hydroxypropionic acid, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, butanediol, 2,3-butanediol, and diethylene glycol.
6. The bio-based polyurethane elastomer according to claim 1, characterized in that The isocyanate is selected from at least one of p-phenylene diisocyanate, m-xylylene diisocyanate, hexamethylene diisocyanate and 1,5-pentamethylene diisocyanate.
7. The bio-based polyurethane elastomer according to claim 1, characterized in that The bio-based chain extender is selected from at least one of 1,6-hexanediol, 1,5-pentanediol, 1,4-butanediol, 1,3-propylene glycol, and ethylene glycol.
8. A method for preparing a bio-based polyurethane elastomer according to any one of claims 1 to 7, the method comprising the following steps: S1. Add the bio-based raw material into a reaction vessel, raise the temperature to 150-200° C., carry out esterification reaction for 2-6 hours, add a catalyst, reduce the pressure to -0.1-0.08 MPa, and terminate the reaction when the hydroxyl value reaches 50-230 mg KOH / g to obtain a bio-based polyester diol; S2. Heat the bio-based polyester diol to 45-90° C., add isocyanate, and react for 2-3 hours; add a chain extender, stir evenly, degas, pour into a mold, hot-press mold at 100-160° C., and mature at 80-130° C. for 12-96 hours to obtain the polyurethane elastomer.
9. A method for degrading a bio-based polyurethane elastomer according to any one of claims 1 to 7, the method comprising the following steps: The polyurethane elastomer sample is crushed and then put into a potassium dihydrogen phosphate / dipotassium hydrogen phosphate solution to prepare a mixed solution, and a degradation enzyme is added to degrade the sample to obtain a degradation solution.
10. The method for degrading a bio-based polyurethane elastomer according to claim 9, characterized in that: The pH of potassium dihydrogen phosphate / dipotassium hydrogen phosphate solution is 6.9 to 7.4; and / or, The degradation temperature is 30 to 60°C; and / or, The mass concentration of the polyurethane elastomer in the mixed solution is 50 to 200 g / L; and / or, The amount of the degrading enzyme used is 0.5 to 2 times the mass of the polyurethane elastomer; and / or, The degrading enzyme is selected from Novozymes non-immobilized lipase A, Novozymes non-immobilized lipase B, porcine pancreatic lipase; and / or, The degradation time is 2 to 40 days.
Citation Information
Patent Citations
Biodegradable unsaturated polyurethane material and preparation method thereof
CN104387553A
Biological-type thermoplastic polyurethane elastomer and preparation method thereof
CN109438653A
Polyurethane elastomer taking bio-based amorphous multi-component polyester as soft segment and preparation method thereof
CN113121786A
Bio-based polyurethane elastomer surgical suture material and preparation method thereof
CN117599231A
High-strength high-elasticity bio-based degradable polyurethane and preparation method thereof