Water-based polyurethane acrylate dispersion, emulsification preparation method thereof and water-based UV (ultraviolet) aluminum powder paint prepared from water-based polyurethane acrylate dispersion
By using low VOC aqueous polyurethane acrylate dispersion in aqueous aluminum powder paint coatings, combining polycarbonate diol and cellulose, the contradiction between storage stability and recoating wear resistance of aqueous aluminum powder paint coatings is solved, and the problem of recoating and wear resistance of aqueous aluminum powder paint coatings is achieved. The effect of improving the recoating performance while ensuring hardness.
Patent Information
- Application Number
- CN202411214446.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-12
AI Technical Summary
Water-based aluminum powder paint coatings have poor stability and insufficient wear resistance in storage and recoating, making it difficult for products on the market to balance the recoating and wear resistance.
Using a low VOC aqueous polyurethane acrylate dispersion, the composition and preparation method are composed of specific raw materials, including adding polycarbonate diol, cellulose and emulsifier to the resin, and emulsifying the process to form a stable aqueous UV aluminum powder paint coating. .
The stability and recoating properties of the coating are significantly improved, ensuring no abnormal settlement at 60°C for 14 days, and showing excellent adhesion and wear resistance on the PC substrate.
Smart Images

Figure BDA0005021143200000021 
Figure BDA0005021143200000022 
Figure BDA0005021143200000031
Abstract
Description
Technical Field
[0001] The invention relates to the field of water-based coatings, more specifically, to the field of resin synthesis emulsification, in particular to the emulsification of resins of water-based UV aluminum paints. Background Art
[0002] It is understood that due to its environmental friendliness, water-based paint has reached a market share of 70% to 80% in the international market, and even 90% in some developed countries. However, this proportion in my country is significantly lower, accounting for only about 10%.
[0003] In recent years, the coatings industry has conducted environmental inspections, requiring coatings companies that fail the inspections to immediately stop production and rectify, and directly requiring coatings companies that cause serious pollution to close, which makes the coatings industry more urgent in terms of the research and development and promotion of water-based coatings. From this perspective, the potential market for water-based low-VOC resins is huge, which is a trend in the future market direction.
[0004] However, compared with oily resins, water-based resins have the disadvantage of poor stability. For example, when aluminum powder paint is prepared with water-based resin, the storage stability of the paint is not enough after adding aluminum powder filler. Therefore, most of the water-based aluminum powder paints on the market currently have poor stability. After being placed for a period of time, the paint will have aluminum powder sedimentation or aluminum powder agglomeration.
[0005] In addition, aluminum powder paint is applied on 3C substrates. Since the preparation process of 3C substrates is complicated and expensive, if defects occur during spraying, the substrate needs to be re-sprayed (re-coated) to cover the defects. Therefore, whether aluminum powder paint can be re-coated is also an important property that the resin needs to have. However, aluminum powder paint products on the market currently cannot balance re-coating performance and wear resistance (RCA) well.
[0006] Therefore, there is an urgent need to develop a water-based aluminum paint resin with good stability, good recoatability and good wear resistance. Summary of the invention
[0007] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a low-VOC aqueous polyurethane acrylate dispersion having excellent stability, recoatability and wear resistance.
[0008] According to one aspect of the present invention, there is provided an aqueous polyurethane acrylate dispersion, comprising the following raw materials in parts by weight:
[0009]
[0010] Preferably, the low-functional acrylic monomer is a difunctional acrylic monomer or a trifunctional acrylic monomer.
[0011] Preferably, the high-functional acrylic monomer is a 6-functional acrylic monomer or a 3-functional acrylic monomer.
[0012] Preferably, the aqueous polyurethane acrylate dispersion of the present invention comprises the following raw materials in parts by weight:
[0013]
[0014] According to another aspect of the present invention, there is provided a method for preparing an aqueous polyurethane acrylate dispersion, comprising:
[0015] The dimethylolpropionic acid, isophorone diisocyanate and polycarbonate diol are reacted at 80° C. for 2 hours, and the reaction is stopped after the NCO is reduced to a certain level. DPHA is added for end-capping. After the NCO is reduced to a certain level, polyurethane acrylate is obtained. After adding 2-functional and 6-functional monomers, cellulose and an emulsifier, triethylamine is used for neutralization, and water and diethylenetriamine chain extender are added for emulsification to obtain the aqueous polyurethane acrylate dispersion according to the present invention.
[0016] According to another aspect of the present invention, there is provided a water-based single-coat UV aluminum paint prepared using the water-based polyurethane acrylate of the present invention, comprising the following raw materials in parts by weight:
[0017]
[0018] Preferably, the water-based aluminum paste is a treated aluminum paste obtained by adding propylene glycol butyl ether and a dispersant and mixing and dispersing them uniformly. After such advance treatment, the aluminum paste is more evenly dispersed in the formula, which is helpful for the coating spraying effect and is also convenient for addition.
[0019] Preferably, the water-based single-coat UV aluminum paint coating comprises the following raw materials in parts by weight:
[0020]
[0021] According to another aspect of the present invention, there is provided a method for preparing a water-based single-coat UV aluminum paint, comprising:
[0022] Dispersing 49 parts by weight of aluminum paste, 49 parts by weight of propylene glycol butyl ether, and 2 parts by weight of a wetting and dispersing agent at 500 r / min for 30 minutes to obtain a treated aluminum paste;
[0023] 2 parts by weight of initiator, 14 parts by weight of treated aluminum paste and 5 parts by weight of water are sequentially added to 100 parts by weight of the aqueous polyurethane acrylate dispersion of the present invention while dispersing at 1000 r / min for 15 minutes, and a suitable amount of thickener is added to adjust the viscosity to obtain a water-based single-coat UV aluminum powder paint.
[0024] Through the solution of the present invention, the following technical effects can be obtained:
[0025] 1. Polycarbonate diol is added to the polyurethane acrylate resin dispersion. Polycarbonate polyol helps the orientation of aluminum paint, has certain resistance, and has excellent adhesion on PC substrate.
[0026] 2. By adding emulsifiers during the emulsification process, the stability of the resin is improved. After being formulated into a water-based UV aluminum paint, the paint has excellent thermal storage stability and can be stored at 60°C for 14 days without abnormalities.
[0027] 3. Low-functional acrylic monomers (such as difunctional acrylic monomers) and cellulose are also added in the emulsification stage. Cellulose can improve the orientation of aluminum powder and also help the adhesion between layers during recoating, thereby improving recoatability and prolonging the recoating time.
[0028] Based on the waterborne polyurethane acrylate dispersion prepared by the above mechanism, a waterborne UV aluminum powder paint is formulated, which effectively solves the problem of the contradiction between storage stability and recoating wear resistance of waterborne UV aluminum powder paint on the market. DETAILED DESCRIPTION
[0029] [Preparation Example]
[0030] 1. Preparation of waterborne polyurethane acrylate dispersion
[0031] The dihydroxymethylpropionic acid, isophorone diisocyanate and polycarbonate diol are reacted at 80°C for 2h, and the reaction is stopped when the NCO content decreases to 3.9%. DPHA is added for end-capping, and the NCO content decreases to 1.3% to obtain polyurethane acrylate. After adding a difunctional (or trifunctional) acrylic monomer and a hexafunctional acrylic monomer, cellulose and an emulsifier are added, and the mixture is neutralized with triethylamine, and then water and a diethylenetriamine chain extender are added for emulsification to obtain an aqueous polyurethane acrylate dispersion.
[0032] According to the component ratios listed in Table 1, the aqueous polyurethane acrylate dispersions of Examples 1 to 5 were prepared (in parts by weight).
[0033] Table 1. Component ratios of aqueous polyurethane acrylate dispersions of Examples 1-4 of the present invention and Comparative Example 1 (parts by weight)
[0034]
[0035]
[0036] Emulsifiers that can be used include one or more of BASF LF221, LF305, LF403, XL50, TO-4070, XP-80, XP-89, and XP-90.
[0037] As the cellulose, one or more of Eastman CAP 482-0.5, CAP 504-0.2, CAB 553-0.4, CAB 531-1, CAB 381-0.1, CAB 381-0.5 and CAB 381-2 can be used.
[0038] The waterborne polyurethane acrylate dispersions of Comparative Examples 2 and 3 are waterborne single-coat UV aluminum paint resin dispersions purchased from other manufacturers.
[0039] 2. Preparation of water-based single-coat UV aluminum paint
[0040] Dispersing 49 parts by weight of aluminum paste, 49 parts by weight of propylene glycol butyl ether, and 2 parts by weight of wetting and dispersing agent BYK192 at 500 r / min for 30 minutes to obtain a treated water-based aluminum paste;
[0041] 2 parts by weight of initiator, 14 parts by weight of treated aluminum paste and 5 parts by weight of water are added in sequence to 100 parts by weight of aqueous polyurethane acrylate dispersion (Examples 1-4 and Comparative Examples 1-3), while dispersing, at 1000 r / min for 15 minutes, and a suitable amount of thickener is added to adjust the viscosity to obtain a water-based single-coat UV aluminum powder paint.
[0042] [Performance test]
[0043] The above water-based single-coat UV aluminum paint was tested for heat storage performance, and the paint film performance was tested after spraying it on the substrate and curing. The specific test performance and test methods are as follows:
[0044] 1. Thermal stability: Seal the above water-based single-coat UV aluminum paint and place it in a 60°C oven for observation. Take it out after 3, 6 and 14 days to observe whether there is caking and precipitation, and conduct spraying test to compare with the paint that has not been thermally stored.
[0045] 2. Spray the above water-based single-coat UV aluminum paint on the PC substrate, control the film thickness to 10-12μm, bake at 60℃ for 15min, and 2 Curing under energy.
[0046] 3. Recoatability: Place the substrate with the sprayed and cured paint film in a 37℃ oven, take it out after 6h, 16h, 24h, 30h, and 48h, and spray it again on the paint film. The baking and curing process remains unchanged. If the adhesion of the paint film after the second spraying is 5B, it can be determined that the aluminum powder paint can be recoated; if the adhesion of the paint film is 4B or lower, it cannot be recoated. The longer the recoatable time, the better the recoatability of the aluminum powder paint.
[0047] 4. Paint film RCA test: Paper tape friction resistance, 175g force, observe whether the cured paint film is worn through and small black spots appear. It should be noted that when comparing RCA results, it is also necessary to pay attention to the recoating time, because RCA and recoating performance are contradictory.
[0048] 5. Paint film pencil hardness: Use a 750g force trolley pencil hardness tester and Mitsubishi pencils of different hardness values to push 5mm on the cured paint film and observe whether there are scratches on the paint film.
[0049] 6. Metallic flash value (FI value): Tested with a multi-angle colorimeter. The instrument data can characterize the metallic texture of aluminum powder paint. The larger the value, the better the metallic texture, and the better the performance of the corresponding aluminum powder paint.
[0050] Table 2. Test results of aluminum powder paint of the embodiments of the present invention and the comparative examples
[0051]
[0052] It can be seen from the above table that the metallic flash value FI of the water-based UV aluminum powder paint prepared in Examples 1-4 of the present invention after curing is much greater than that of the aluminum powder paint in the comparative example, that is, the metallic texture of the water-based UV aluminum powder paint according to the scheme of the present invention is better than that of the aluminum powder paint in the prior art.
[0053] The water-based UV aluminum powder paint prepared according to the embodiment of the present invention has good stability. Although a small amount of aluminum powder settles, it can be stirred back and sprayed without abnormality, so the stability is good. In contrast to the present invention, the aluminum powder paints of Comparative Examples 2-3 all gel and become solid after 14 days of hot storage and cannot be stirred. However, no emulsifier is added to the formula of Comparative Example 1, and its stability effect is not good, which can indicate that the addition of an emulsifier in the emulsification stage is helpful for the stability of the aluminum powder paint.
[0054] The aluminum powder paints of Examples 1-4 of the present invention are all recoatable, and the recoatable time of the aluminum powder paints of Examples 2 and 3 is more than 30 hours, and the aluminum powder paint of Example 3 even reaches a recoatable time of 48 hours, which is very good recoatability. In comparison, the recoatable time of Comparative Examples 2 and 3 is 0, and they are not recoatable.
[0055] There is a contradiction between the hardness of the paint film after curing and the recoatability of the paint. From the test results of wear resistance in the above table, it can be seen that the aluminum paint with low wear resistance RCA has high recoatability. However, the aluminum paints of Comparative Examples 2 and 3 have particularly high RCA and poor recoatability (recoat time is 0).
[0056] As the amount of cellulose increases, the wear resistance RCA will decrease and the recoating performance will increase. The aluminum powder paint of Example 3 of the present invention has the longest recoating time. This is because the aluminum powder paint formula of Example 3 has a large amount of cellulose added, resulting in a low RCA, but cellulose can improve the orientation of aluminum powder and increase the surface roughness of the paint film, which can help the adhesion between layers during recoating, and correspondingly improve the recoating performance, and the recoating time can be long.
[0057] In short, there is a contradiction between hardness and recoatability. The product of the present invention maximizes recoatability while ensuring hardness as much as possible, that is, it takes both hardness and recoatability into consideration.
[0058] Although embodiments of the present invention are described in detail herein, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A waterborne polyurethane acrylate dispersion, comprising the following raw materials in parts by weight:
2. The aqueous polyurethane acrylate dispersion according to claim 1, wherein The low-functional acrylic monomer is a difunctional acrylic monomer or a trifunctional acrylic monomer.
3. The aqueous polyurethane acrylate dispersion according to claim 1, wherein The high-functional acrylic monomer is a 6-functional acrylic monomer or a 3-functional acrylic monomer.
4. The aqueous polyurethane acrylate dispersion according to claim 1, comprising the following raw materials in parts by weight:
5. A method for preparing the aqueous polyurethane acrylate dispersion according to claim 1, comprising: Dimethylolpropionic acid, isophorone diisocyanate and polycarbonate diol are reacted at 80°C for 2 hours, and the reaction is stopped after the NCO is reduced to a certain level. DPHA is added for end-capping. After the NCO is reduced to a certain level, polyurethane acrylate is obtained. After adding difunctional and hexafunctional monomers, cellulose and an emulsifier, triethylamine is used for neutralization, and water and diethylenetriamine chain extender are added for emulsification to obtain an aqueous polyurethane acrylate dispersion.
6. A water-based single-coat UV aluminum paint, comprising the following raw materials in parts by weight: 40-120 parts of the aqueous polyurethane acrylate dispersion according to any one of claims 1 to 4; 7. The water-based single-coat UV aluminum paint according to claim 6, wherein: The water-based aluminum paste is a treated aluminum paste obtained by adding propylene glycol butyl ether and a wetting dispersant into the aluminum paste and mixing and dispersing the mixture uniformly.
8. The water-based single-coat UV aluminum paint according to claim 6, wherein: By weight, it contains the following raw materials: 60-100 parts of the aqueous polyurethane acrylate dispersion according to any one of claims 1 to 4; 9. A method for preparing the water-based single-coat UV aluminum paint according to claim 6, comprising: Dispersing 49 parts by weight of aluminum paste, 49 parts by weight of propylene glycol butyl ether, and 2 parts by weight of a wetting and dispersing agent at 500 r / min for 30 minutes to obtain the treated aluminum paste; 2 parts by weight of initiator, 14 parts by weight of treated aluminum paste and 5 parts by weight of water are sequentially added to 100 parts by weight of the aqueous polyurethane acrylate dispersion while dispersing at 1000 r / min for 15 minutes, and a suitable amount of thickener is added to adjust the viscosity to obtain the aqueous single-coat UV aluminum powder paint.