Curing accelerator for epoxy resin, preparation method of curing accelerator, coating composition containing curing accelerator and application of curing accelerator
By introducing new curing accelerators containing carboxyl groups, tertiary amines and alcohol hydroxyl groups into the epoxy resin system, the problems of limited effect and poor yellowing resistance are solved, and faster curing speed and better Yellowing resistance and the accelerator is a colorless liquid, which is easy to operate.
Patent Information
- Application Number
- CN202411177749.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The accelerators of the existing epoxy-amine system are limited in effect. Commonly used phenols and carboxylic acid accelerators are solids at room temperature and need to be dissolved at high temperature. The curing agents produced are prone to turn red, and the tertiary amine accelerators have a large odor and are resistant to yellowing. The variable performance is poor and there is a lack of effective research solutions.
A new epoxy resin curing accelerator containing carboxyl groups, tertiary amines and alcohol hydroxyl groups is prepared by reaction of alicyclic acid anhydrides with alcohol amines containing tertiary amine groups. It has a colorless liquid at room temperature and is at 80°C to The reaction was produced at 120°C, combined with inert gas protection, and was used to prepare the coating composition to improve curing speed and yellowing resistance.
It provides higher curing promotion effect, faster curing speed, low odor and better yellowing resistance, easy to operate, and the accelerator is a colorless liquid, which is easy to mix into the formula system.
Smart Images

Figure CN118930818A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin curing agents, in particular to a curing accelerator containing carboxyl groups, tertiary amines and alcoholic hydroxyl groups and a preparation method thereof, and a coating composition prepared by using the curing accelerator as a raw material and the application thereof. Background Art
[0002] As one of the currently common thermosetting resin systems, epoxy resin is widely used in adhesives, coatings, composite materials and other fields due to its outstanding mechanical strength, adhesion, dielectric properties, solvent resistance, heat resistance and low shrinkage properties of the cured product. Among them, the epoxy-amine system accounts for a high proportion in the entire epoxy resin field due to its convenient operation and flexible curing process.
[0003] In order to increase the curing speed of epoxy-amine systems and shorten the process time, it is usually necessary to add accelerators to the epoxy-amine formula system to increase the degree of reaction. However, over the long term, the accelerators of epoxy-amine systems have not been well developed. Currently, the commonly used epoxy-amine accelerators are mostly phenols, carboxylic acids, and tertiary amines. The promotion effect of a single type of accelerator is limited. At the same time, commonly used phenols (phenol, bisphenol A, o-cresol, etc.) and carboxylic acids (salicylic acid, etc.) are solid at room temperature and need to be dissolved in solvents under high temperature conditions. At the same time, the curing agent produced by them is easy to turn red; and the commonly used tertiary amines (DMP-10, DMP-30) have a strong smell and poor yellowing resistance. At present, there is no technology at home and abroad to study this direction. Summary of the invention
[0004] In order to solve the above-mentioned problems existing in the accelerator during the epoxy-amine curing reaction, the present invention provides a novel accelerator containing carboxyl, tertiary amine and alcoholic hydroxyl groups at the same time, a preparation method thereof, and a coating composition containing the same and application thereof.
[0005] In order to achieve the purpose of the present invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a curing accelerator for epoxy resin, which has a general structure as shown in Formula I:
[0007]
[0008] Among them, R 1 Select from -H or C 1 -C 3 Alkyl, for example, -H, methyl, ethyl, propyl, preferably -H and methyl;
[0009] R 2 Selected from C 1 -C 5 Alkylene, such as -CH2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 CH 2 , preferably C 2 -C 3 of alkylene;
[0010] R 3 Selected from C 1 -C 4 Alkyl groups, such as -CH 3 、-CH 2 CH 3 、-CH 2 CH 2 CH 3 、-CH 2 CH 2 CH 2 CH 3 , preferably C 1 -C 3 The alkyl group;
[0011] R 4 Selected from C 1 -C 5 Alkylene, such as -CH 2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 CH 2 -, preferably C 2 -C 3 of alkylene.
[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned epoxy resin curing accelerator, comprising:
[0013] The alicyclic acid anhydride having a structure shown in Formula II and the alcohol amine having a tertiary amine group having a structure shown in Formula III are reacted in a certain ratio to obtain the curing accelerator for the epoxy resin;
[0014]
[0015] Among them, R 1 Select from -H or C 1 -C 3 Alkyl, for example, -H, methyl, ethyl, propyl, preferably -H and methyl;
[0016] R 2 Selected from C 1 -C 5 Alkylene, such as -CH 2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 CH 2 -, preferably C 2 -C 3 of alkylene;
[0017] R 3 Selected from C 1 -C 4 Alkyl groups, such as -CH 3 、-CH 2 CH 3 、-CH 2 CH 2 CH 3 、-CH 2 CH 2 CH 2 CH 3 , preferably C 1 -C 3 The alkyl group;
[0018] R 4 Selected from C 1 -C 7 Alkylene, such as -CH 2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2-、-CH 2 CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 CH 2 -, preferably C 2 -C 3 of alkylene.
[0019] In some specific embodiments, the molar ratio of the alicyclic anhydride to the alcoholamine containing a tertiary amine group is 1:(1.0-1.1), preferably 1:(1.0-1.05).
[0020] In some specific embodiments, the alicyclic anhydride is slowly added dropwise to the alcoholamine containing a tertiary amine group under stirring. The stirring state can preferably be carried out at a speed of 200 r / min to 500 r / min, more preferably 250 r / min to 350 r / min, for example, 280 r / min, 300 r / min, 320 r / min.
[0021] In some specific embodiments, the above reaction is carried out at 80° C. to 120° C., preferably 90° C. to 110° C., for example, 95° C., 100° C., 105° C. Specifically, the reaction time is 2 to 4 hours, preferably 3 to 4 hours.
[0022] In some preferred embodiments, the reaction is carried out under the protection of an inert gas, wherein the inert gas is selected from nitrogen and argon, and is preferably carried out in a nitrogen atmosphere.
[0023] The present invention provides a coating composition for yellowing-resistant floor surface coating in a third aspect, the coating composition comprising component A and component B, wherein component A comprises liquid epoxy resin and epoxy reactive diluent; component B comprises alicyclic diamine, curing accelerator and auxiliary agent, wherein the auxiliary agent comprises dispersant and defoamer;
[0024] Wherein, the curing accelerator is the above-mentioned curing accelerator for epoxy resin or the curing accelerator for epoxy resin prepared by the above-mentioned method.
[0025] In some specific embodiments, based on the mass fractions of each component in component A (the total mass fractions are 100), component A includes:
[0026] 85-100 parts of liquid epoxy resin, preferably 90-95 parts;
[0027] 0 to 15 parts of epoxy reactive diluent, preferably 5 to 10 parts;
[0028] Calculated by the mass fraction of each component in component B (the total mass fraction is 100), component B includes:
[0029] 60 to 80 parts of alicyclic diamine, preferably 64 to 79 parts;
[0030] 5 to 35 parts of benzyl alcohol, preferably 9 to 28 parts;
[0031] 5 to 15 parts, preferably 8 to 12 parts, of a curing accelerator for epoxy resin;
[0032] Dispersant 0.1 to 1 part, preferably 0.2 to 0.6 part;
[0033] The defoaming agent is 0.2 to 2 parts, preferably 0.4 to 0.7 parts.
[0034] In some specific embodiments, the preparation method of the component A is: mixing a liquid epoxy resin and an epoxy reactive diluent to obtain the component A;
[0035] The preparation method of the B component is as follows: alicyclic diamine, benzyl alcohol, epoxy resin curing accelerator, dispersant and defoamer are mixed to obtain the B component.
[0036] In some specific embodiments, the liquid epoxy resin is selected from bisphenol A epoxy resin, preferably 128 epoxy resin.
[0037] The epoxy reactive diluent is selected from phenyl glycidyl ether, cresyl glycidyl ether, benzyl glycidyl ether, C 12 -C 14 One or more of glycidyl ether or butyl glycidyl ether;
[0038] The alicyclic diamine is selected from one or more of diaminodicyclohexylmethane, isophoronediamine, 1,3-cyclohexanedimethylamine or 1,2-cyclohexanediamine; in some preferred embodiments, it is diaminodicyclohexylmethane and / or isophoronediamine;
[0039] The dispersant is selected from one or more of fatty acid derivative dispersants, aliphatic amide dispersants and ester dispersants, preferably a fatty acid dispersant, such as Tego Dispers 610 and / or Dispers 630.
[0040] The defoamer is selected from one or more of polyether defoamers, silicone defoamers and alcohol defoamers; preferably silicone defoamers, such as BYK066N and / or BYKA530.
[0041] In a fourth aspect, the present invention further provides a method for preparing a yellowing-resistant epoxy floor topcoat using the above-mentioned coating composition, wherein component A and component B are mixed in a mass ratio of 100:(30-35) and then cured.
[0042] In some specific embodiments, component A and component B are mixed in a mass ratio of 100:(31-33), for example, 100:32.
[0043] The above technical solution has the following technical effects:
[0044] Compared with traditional carboxylic acid (salicylic acid) and phenolic accelerators (phenol, bisphenol A, etc.), the epoxy resin curing accelerator provided by the present invention contains a carboxylic acid group, a tertiary amine group and a hydroxyl group in its structure, has a higher accelerating effect, and yellowing resistance; at the same time, the accelerator provided by the present invention is a colorless liquid at room temperature, is more convenient to use, and is easier to mix into the formulation system.
[0045] The yellowing-resistant epoxy floor topcoat provided by the invention has faster curing speed, lower odor and more excellent yellowing-resistant performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 : Infrared spectrum of the epoxy resin curing accelerator obtained in the embodiment of the present invention. DETAILED DESCRIPTION
[0047] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0048] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0049] The following implementations are tested using the following methods:
[0050] (1) Curing agent color: Use Shimadzu UV-1201V spectrophotometer for color testing;
[0051] (2) Curing agent viscosity: tested using BrookField viscometer DV2T, test conditions: 25°C, No. 28 rotor;
[0052] (3) Operation time: the time for drawing 100g of AB mixture at 25°C;
[0053] (4) Surface drying time: the time it takes for a 3 mm thick paint film to stop sticking to the touch at 25°C;
[0054] (5) Hardness of cured product: The hardness data is obtained by testing 10 g of AB mixture in a disposable plastic cup at 25°C for 24 h using a Shore D hardness tester.
[0055] (6) Yellowing resistance test: After the 3 mm thick paint film is cured for 7 days, it is irradiated under a 60W UV lamp for 1 hour to observe the color change of the paint film.
[0056] Source of raw materials:
[0057]
[0058] Example 1
[0059] 119 g of N-methyldiethanolamine was added to a 500 ml three-necked flask, nitrogen was introduced into the three-necked flask and mechanical stirring was started. Under the condition of stirring speed of 250 r / min, the material was heated to 90° C. using an oil bath; then 168 g of methylhexahydrophthalic anhydride was weighed and slowly added dropwise to the three-necked flask. After reacting for 3 hours, a curing accelerator AC-1 for epoxy resin containing a carboxylic acid group, a tertiary amine group and an alcoholic hydroxyl group as shown in the following formula was obtained.
[0060]
[0061] The accelerator AC-1 obtained by the above method was subjected to infrared analysis. The analysis results are shown in the attached Figure 1 As shown in the spectrum, 1820cm -1 The anhydride C=O absorption peak and 1300~1200cm -1 The disappearance of the COC stretching vibration absorption peak at 3300-2500cm -1 The appearance of the associative -OH stretching vibration absorption peak of the carboxylic acid at the position indicates that N-methyldiethanolamine reacts with methylhexahydrophthalic anhydride in the system, and the reaction of methylhexahydrophthalic anhydride is complete.
[0062] Example 2
[0063] 139.65 g of N-ethyldiethanolamine was added to a 500 ml three-necked flask, nitrogen was introduced into the three-necked flask and mechanical stirring was started. Under the condition of stirring speed of 350 r / min, the material was heated to 110° C. using an oil bath; then 154 g of 1,2-cyclohexanedicarboxylic anhydride was weighed and slowly added dropwise to the three-necked flask. After reacting for 4 hours, a curing accelerator AC-2 for epoxy resin containing a carboxylic acid group, a tertiary amine group and an alcoholic hydroxyl group as shown in the following formula was obtained.
[0064]
[0065] The accelerator AC-2 obtained by the above method was subjected to infrared analysis, and its spectrum was similar to that of Example 1.
[0066] Example 3
[0067] 75.7 g of N-propyldiethanolamine and 75.7 g of 3-(3-hydroxypropylamino)-1-propanol were added to a 500 ml three-necked flask, nitrogen was introduced into the three-necked flask and mechanical stirring was started. Under the condition of stirring speed of 350 r / min, the materials were heated to 110° C. in an oil bath; then 154 g of 1,2-cyclohexanedicarboxylic anhydride was weighed and slowly added dropwise to the three-necked flask. After reacting for 4 hours, a curing accelerator AC-3 for epoxy resin containing a carboxylic acid group, a tertiary amine group and an alcoholic hydroxyl group as shown in the following formula was obtained.
[0068]
[0069] The accelerator AC-3 obtained by the above method was subjected to infrared analysis, and its spectrum was similar to that of Example 1.
[0070] Example 4
[0071] 147 g of 3-[(2-hydroxyethyl)methylamino]-1-propanol was added to a 500 ml three-necked flask, nitrogen was introduced into the three-necked flask and mechanical stirring was started. Under the condition of stirring speed of 320 r / min, the materials were heated to 100° C. in an oil bath; then 84 g of methylhexahydrophthalic anhydride and 77 g of 1,2-cyclohexanedicarboxylic anhydride were weighed and heated to 50° C. to melt into liquid, and then slowly added dropwise to the three-necked flask. After reacting for 3.8 hours, a curing accelerator AC-4 for epoxy resin containing a carboxylic acid group, a tertiary amine group and an alcoholic hydroxyl group as shown in the following formula was obtained.
[0072]
[0073] The accelerator AC-4 obtained by the above method was subjected to infrared analysis, and its spectrum was similar to that of Example 1.
[0074] Example 5
[0075] In a 500ml three-necked flask, 59.5g of N-methyldiethanolamine and 66.5g of N-ethyldiethanolamine were placed. Nitrogen was introduced into the three-necked flask and mechanical stirring was started. Under the condition of stirring speed of 305r / min, the materials were heated to 95°C using an oil bath. Then, 84g of methylhexahydrophthalic anhydride and 77g of 1,2-cyclohexanedicarboxylic anhydride were weighed and heated to 50°C to melt into liquid, and then slowly added dropwise to the three-necked flask. After reacting for 3.8h, a curing accelerator AC-5 for epoxy resin containing a carboxylic acid group, a tertiary amine group and an alcoholic hydroxyl group as shown in the following formula was obtained.
[0076]
[0077] The accelerator AC-5 obtained by the above method was subjected to infrared analysis, and its spectrum was similar to that of Example 1.
[0078] The basic properties of the epoxy resin curing accelerator obtained above and conventional accelerators salicylic acid, bisphenol A and DMP-30 were tested. The test data are shown in Table 1 below:
[0079] Table 1
[0080]
[0081] According to the data in Table 1 above, it can be seen that compared with salicylic acid and bisphenol A solid accelerators, the accelerators AC-1 to AC-5 obtained in the examples of the present invention are low-viscosity liquids at room temperature and have better operation convenience. At the same time, compared with the currently commonly used DMP-30 accelerator, the accelerator obtained in the present invention has lower odor, viscosity and better color.
[0082] The epoxy resin curing accelerator is used to prepare a coating composition according to the following formula ratio, as shown in the following table:
[0083] Component A contains:
[0084] composition Mass fraction NPEL128 liquid epoxy resin 93 <![CDATA[C 12 -C 14 Glycidyl ether]]> 7
[0085] Component B contains:
[0086] composition Mass fraction Diaminodicyclohexylmethane 79 Benzyl alcohol 12 Curing accelerator for epoxy resin 8 Tego Dispers 610 0.5 BYK066N Defoamer 0.5
[0087] By using different types of accelerators, the materials in the above-mentioned component A and component B are mixed at room temperature according to the ratio, and after uniform mixing, component A and component B containing different accelerators are obtained.
[0088] After mixing in a mass ratio of 100:32 and then curing, a yellowing-resistant epoxy floor coating is obtained.
[0089] The above-obtained B components containing different accelerators and the obtained epoxy floor topcoat were subjected to performance tests, and the test data are shown in Tables 2 and 3 below:
[0090] Table 2
[0091]
[0092]
[0093] Table 3
[0094]
[0095] It can be seen from the comparative data of Tables 2 and 3 that, compared with commonly used accelerators (salicylic acid, bisphenol A, DMP-30, etc.), the curing agent prepared by the accelerator containing carboxylic acid groups, tertiary amine groups and alcoholic hydroxyl groups provided by the present invention has a shorter operation time and surface drying time, higher hardness and better yellowing resistance effect; at the same time, the accelerator provided by the present invention is a colorless and odorless liquid at room temperature, has more convenient operation performance, and has better yellowing resistance.
Claims
1. A curing accelerator for epoxy resin, characterized in that The epoxy resin curing accelerator has a general structure as shown in Formula I: Wherein, R1 is selected from -H or C1-C3 alkyl, preferably -H and methyl; R2 is selected from C1-C5 alkylene, preferably C2-C3 alkylene; R3 is selected from C1-C4 alkyl, preferably C1-C3 alkyl; R4 is selected from C1-C5 alkylene, preferably C2-C3 alkylene.
2. A method for preparing the epoxy resin curing accelerator according to claim 1, characterized in that: The method comprises: The alicyclic acid anhydride having a structure shown in Formula II and the alcohol amine having a tertiary amine group having a structure shown in Formula III are reacted in a certain ratio to obtain the curing accelerator for the epoxy resin; Wherein, R1 is selected from -H or C1-C3 alkyl, preferably -H and methyl; R2 is selected from C1-C5 alkylene, preferably C2-C3 alkylene; R3 is selected from C1-C4 alkyl, preferably C1-C3 alkyl; R4 is selected from C1-C5 alkylene, preferably C2-C3 alkylene.
3. The method according to claim 2, characterized in that The molar ratio of the alicyclic anhydride to the alcoholamine containing a tertiary amine group is 1:(1.0-1.1), preferably 1:(1.0-1.05); Preferably, the alicyclic anhydride is slowly added dropwise to the alcoholamine containing a tertiary amine group under stirring, and the stirring is preferably carried out at a speed of 200 r / min to 500 r / min, more preferably 250 r / min to 350 r / min.
4. The method according to claim 2 or 3, characterized in that: The reaction is carried out at 80°C to 120°C, preferably 90°C to 110°C; The reaction time is 2 to 4 hours, preferably 3 to 4 hours; More preferably, the reaction is carried out under the protection of an inert gas, wherein the inert gas is selected from nitrogen and argon, preferably nitrogen.
5. A coating composition, characterized in that: The coating composition comprises component A and component B, wherein component A comprises liquid epoxy resin and epoxy reactive diluent; component B comprises alicyclic diamine, curing accelerator and auxiliary agent, wherein the auxiliary agent comprises dispersant and defoamer; Wherein, the curing accelerator is the curing accelerator for epoxy resin according to claim 1 or the curing accelerator for epoxy resin prepared by the method described in any one of claims 2 to 4.
6. The coating composition according to claim 5, characterized in that In parts by mass, in component A: 85-100 parts of liquid epoxy resin, preferably 90-95 parts; 0 to 15 parts of epoxy reactive diluent, preferably 5 to 10 parts; In parts by mass, in component B: 60 to 80 parts of alicyclic diamine, preferably 64 to 79 parts; 5 to 35 parts of benzyl alcohol, preferably 9 to 28 parts; 5 to 15 parts, preferably 8 to 12 parts, of a curing accelerator for epoxy resin; Dispersant 0.1 to 1 part, preferably 0.2 to 0.6 part; The defoaming agent is 0.2 to 2 parts, preferably 0.4 to 0.7 parts.
7. The coating composition according to claim 6, characterized in that The preparation method of the A component is: mixing a liquid epoxy resin and an epoxy reactive diluent to obtain the A component; The preparation method of the B component is as follows: alicyclic diamine, benzyl alcohol, epoxy resin curing accelerator, dispersant and defoamer are mixed to obtain the B component.
8. The coating composition according to claim 6 or 7, characterized in that The liquid epoxy resin is selected from bisphenol A type epoxy resin, preferably 128 type epoxy resin; The epoxy reactive diluent is selected from phenyl glycidyl ether, cresyl glycidyl ether, benzyl glycidyl ether, C 12 -C 14 One or more of glycidyl ether or butyl glycidyl ether; The alicyclic diamine is selected from one or more of diaminodicyclohexylmethane, isophoronediamine, 1,3-cyclohexanedimethylamine or 1,2-cyclohexanediamine; preferably diaminodicyclohexylmethane and / or isophoronediamine; The dispersant is selected from one or more of fatty acid derivatives, aliphatic amides and esters, preferably fatty acids; The defoamer is selected from one or more of polyethers, silicones and alcohols; preferably silicone defoamers.
9. A use of the coating composition according to any one of claims 5 to 8 for preparing yellowing-resistant epoxy floor topcoat, characterized in that: Component A and component B are mixed in a mass ratio of 100:(30-35) and then cured to form a yellowing-resistant epoxy floor coating.
10. The use according to claim 9, characterized in that Component A and component B are mixed in a mass ratio of 100:(31-33).
Citation Information
Patent Citations
Application of aryl alcohol amine as epoxy resin diluent and epoxy resin composition
CN114854089A
High molecular weight polyimide epoxy resin, preparation method and application thereof
CN116655866A
Colorless and transparent epoxy composition with high UV yellowing resistance and preparation method thereof
CN117343479A
Epoxy resin composition
JP1999060696A