High-elasticity polyoxamide as well as preparation method and application thereof

By using polyether chains and oxalamide structures to form highly elastic polyoxalamide, the toxicity and production hazards of diisocyanate compounds in the prior art are solved, and the efficient preparation and excellent performance of high elastic fibers are achieved.

CN118930849AActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310538472.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

The diisocyanate compounds used in existing elastic fibers are highly toxic and dangerous in production, making it difficult to develop highly elastic fibers.

Method used

Polyether chains are used as soft segments and oxalamide structures are used as hard segments. The reaction of oxalic acid and/or oxalic acid diesters with diamines forms a highly elastic polyoxalamide to form a linear block copolymer, avoiding the use of highly toxic diisocyanate compounds .

Benefits of technology

The preparation of high elastic fibers is achieved, with high elongation of break, fracture strength and excellent elastic recovery. The preparation process is simple and the raw materials are stable, which avoids the use of highly toxic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930849A_ABST
    Figure CN118930849A_ABST
Patent Text Reader

Abstract

The invention discloses high-elasticity polyoxamide and a preparation method and application thereof.According to the high-elasticity polyoxamide, a polyether chain is adopted for providing a soft segment, an oxamide structure and a six-membered rigid ring are adopted for providing a hard segment, a soft-hard embedded linear structure is formed, and the polyoxamide is endowed with high elasticity; specifically, the molecular structure of the high-elasticity polyoxamide contains a polyether chain structural unit and an oxamide structural unit as shown in the formula (I): # imgabs0 #, R'is a group containing a six-membered rigid ring, and fibers prepared from the high-elasticity polyoxamide have high elongation at break, high breaking strength, high 200% stress and excellent elastic recovery rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical materials and relates to a high-elastic polyoxamide and a preparation method and application thereof. Background Art

[0002] Elastic fibers are generally linear block copolymers composed of soft segments and hard segments. The soft segments can be stretched and connected to each other by hard segments. The alternation of soft and hard segments is equivalent to forming a series of small springs (such as Figure 1 As shown). In the aggregate structure of multiple molecules of elastic fiber, the soft segment can move freely after being stressed at room temperature, and the force between molecular chains is very weak. The hard segment forms entanglement and cross-linking. The soft segment can move like a spring, which is equivalent to weaving many small springs into a fishing net. It has both elasticity and can be pulled back and contracted by the hard segment.

[0003] The hard segments in elastic fibers contain a variety of polar groups, are crystalline, and can produce transverse cross-links between macromolecular chains. Under the action of stress, this segment basically does not deform, thus preventing slippage between molecules, providing the necessary node conditions for the large-scale elongation and rebound of the soft segment, and giving the fiber a certain strength. It is this coexistence system of soft and hard segments that leads to the high elasticity of elastomers, such as spandex fibers (Wang Jiazhao, Sun Zongxuan, Ji Yongling. Production and Application of Spandex Elastic Yarn, Beijing: Textile Industry Press, 1989).

[0004] To obtain ultra-high elastic fibers, the soft segment must not easily enter the lattice formed by the hard segment, that is, the hard segment must have an increased polarity, and the hard segments form crystals through hydrogen bonds or strong polar bonds, while the soft segment must form an independent system with low polarity. The hard segment and the soft segment are two independent systems that do not interfere with each other. To achieve this goal, the soft segment and the hard segment must be fully expanded respectively, making the hard segment harder and the soft segment softer, each performing its own function and "separating". Since the crystalline region and the non-crystalline region belong to the microstructure of the fiber, it is called "microphase separation". Microphase separation means that at room temperature, the hard segment microregion is not soluble in the soft segment, but is distributed in the soft segment, playing a cross-linking role, which has a great impact on the performance of polyurethane products. It is the key to spandex's ultra-high elasticity (Tao Can, Microphase Separation Structure Regulation, Performance and Application of Polyurethane, Anhui University, 2018; You Gexin, Chen Xiri, Yang Bo, Zhou Xiuwen. Effect of Soft Segment Molecular Weight on Microphase Separation Degree and Tensile Properties of Spandex, Engineering Plastics Application. 2017.12:88-92; P, Bagdi K, Molnár K, et al. Quantitative mapping of elastic moduli at the nanoscale in phase separated polyurethanes by AFM. European Polymer Journal, 2011, 47(4): 692-698).

[0005] The elastic fiber most involved in the existing technology is spandex fiber. The "softblock" in the spandex molecular structure mainly comes from polyethers, such as poly-1,4-butylene glycol (PTMEG), poly-1,2-propylene glycol, and even polyethylene glycol, and aliphatic polyesters, such as polybutylene succinate, polycaprolactone, etc.; the "hard segment" in the spandex molecular structure depends on the isocyanate functional groups formed by toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI) and alcohol, and the urea functional groups with organic amine properties. Their strong intermolecular hydrogen bonds and rigidity provide:

[0006]

[0007] Although diisocyanate compounds can be the "hard block" in spandex fiber molecules, the raw material diisocyanate compounds are highly toxic and very sensitive, and are too reactive to water, amines and other compounds. The preparation process of the raw material requires the use of phosgene, a highly toxic compound, and the production risk factor is extremely high. Therefore, it is urgent to develop a new high-elastic fiber. Summary of the invention

[0008] In order to overcome the problems existing in the prior art, the present invention provides a highly elastic polyoxamide and a preparation method and application thereof, wherein a polyether chain is used to provide a "soft segment", an oxamide structure (i.e., obtained by reacting oxalic acid and / or oxalic acid diester with diamine) and a six-membered rigid ring provide a "hard segment" to form the highly elastic polyoxamide.

[0009] One of the objects of the present invention is to provide a highly elastic polyoxamide, the molecular structure of which contains a polyether chain structural unit and an oxamide structural unit represented by formula (I):

[0010]

[0011] Wherein, R' is a group containing a rigid six-membered ring.

[0012] The polyether chain is used as a soft segment, and the structural unit shown in formula (I) is used as a hard segment, forming a linear block copolymer composed of a soft segment and a hard segment.

[0013] The polyoxamide described in the present invention refers to polyoxamide obtained by polymerization of oxalic acid and / or oxalic acid diester with diamine substances. Due to the presence of two adjacent amide groups in its structure, polyoxamide has a large number of intermolecular hydrogen bonds and extremely high cohesive energy density, great rigidity, melting point and solvent resistance. The hydrogen bonding between the oxamide functional groups is shown below:

[0014]

[0015] The oxamide structural unit of the present invention contains not only an oxamide rigid structure, but also an R' rigid structure, that is, the polyoxamide structure of the present invention contains a dioxamide structure formed by a rigid six-membered ring (such as an aromatic diamine or a cyclic dipeptide diamine compound). Compared with the ordinary aliphatic dioxamide structure, the present invention has better polarity and rigidity, and can better play the role of "hard block" in the elastic macromolecular chain.

[0016] In a preferred embodiment, R' is a group containing a rigid six-membered ring, and the rigid six-membered ring is at least one of a cyclohexyl ring, a benzene ring, and a 2,5-diketopiperazine ring.

[0017] In a further preferred embodiment, R' is selected from one of the structures represented by formula (I-1) to formula (I-6), preferably one of the structures represented by formula (I-1) to formula (I-4):

[0018]

[0019] In formula (I-1) to formula (I-4), R1 to R7 are each independently selected from hydrogen, alkyl or aryl, preferably from hydrogen, C1 to C10 alkyl or C6 to C10 aryl, more preferably from hydrogen or C1 to C6 alkyl; R8 to R9 are each independently selected from alkylene or arylene, preferably from C1 to C10 alkylene or C6 to C10 arylene, more preferably from C1 to C6 alkylene.

[0020] Among them, the C1~C10 can be C1, C2, C4, C6, C8 or C10, the C6~C10 can be C6, C7, C8, C9 or C10, and the C1~C6 can be C1, C2, C3, C4, C5 or C6.

[0021] In a further preferred embodiment, R' is selected from one of the following structures:

[0022]

[0023] In a further preferred embodiment, R' is selected from one of the following structures:

[0024]

[0025] In a preferred embodiment, the molecular structure of the highly elastic polyoxamide contains a repeating structural unit represented by formula (II):

[0026]

[0027] In formula (II), R' has the same definition as in formula (I), Represents a polyether chain.

[0028] Wherein, the soft segment in formula (II) is a polyether chain, and the hard segment is shown in the dotted box in the following formula:

[0029]

[0030] If the hard segment structure consists only of The hard segment structure has a small molecular weight, small polarity, small rigidity and small intermolecular force. It is not easy to form microphase separation in the polyether soft segment of polyetheramine by simply relying on it as a hard segment. The hard segment structure provided by the present invention (as shown in the dotted line frame in the above formula) is a structure that connects two The connection forms a new hard segment structure, which has a large molecular weight, high polarity, strong rigidity and intermolecular force, is easier to crystallize, and can produce lateral cross-linking between macromolecular chains, and has higher resilience.

[0031] In a preferred embodiment, the polyether chain is a polyether chain with a molecular weight of 300 to 3000, preferably a polyether chain with a molecular weight of 600 to 2000, for example, a molecular weight of 300, 500, 700, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800 or 3000.

[0032] In a further preferred embodiment, the polyether in the polyether chain is at least one of a homopolymer, a copolymer of two or three of polyoxyethylene, polyoxypropylene and polytetrahydrofuran, for example, at least one of polyoxyethylene, polyoxypropylene, a polyoxyethylene-polyoxypropylene copolymer or polytetrahydrofuran.

[0033] In a preferred embodiment, the highly elastic polyoxamide is selected from at least one of the polymers represented by the following formula (III):

[0034]

[0035] In formula (III), R' has the same definition as in formula (I), represents a polyether chain, and in the above formula, n is 2 to 100, for example, 2, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90 or 100.

[0036] In the present invention, the polyoxamide has a soft segment and a hard segment, such as Figure 1 As shown, Represents the soft block, i.e. the polyether segment, It represents a hard block, i.e., an oxalamide segment, thus forming a linear structure of soft and hard interlocking, giving the polyoxalamide high elasticity.

[0037] In a preferred embodiment, the highly elastic polyoxamide is prepared from raw materials including polyetheramine, oxalic acid and / or oxalic acid diester, and small molecule diamine compounds.

[0038] The preparation process does not involve the use of highly toxic diisocyanate compounds.

[0039] The second object of the present invention is to provide a method for preparing highly elastic polyoxamide, preferably for preparing the highly elastic polyoxamide described in one of the objects of the present invention, the preparation method comprising: reacting raw materials including polyether amine, oxalic acid and / or oxalic acid diester, and small molecule diamine compounds to obtain the same.

[0040] In a preferred embodiment, the molecular weight of the polyetheramine is 300-3000, preferably 600-2000, for example 300, 500, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800 or 3000.

[0041] In a further preferred embodiment, the polyetheramine is a terminal difunctional polyetheramine, wherein the polyether is at least one of a homopolymer, a copolymer of two or three of polyoxyethylene, polyoxypropylene and polytetrahydrofuran, for example, at least one of polyoxyethylene, polyoxypropylene, a polyoxyethylene-polyoxypropylene copolymer or polytetrahydrofuran.

[0042] In a further preferred embodiment, the polyetheramine may be: CAED-600, CAED-900, CAD-2000, CAED-2003 produced by Yangzhou Chenhua New Materials Co., Ltd., or CAED-600, CAED-900, CAD-2000, CAED-2003 produced by Huntsman Corporation. D-230, D-400, D-2000, D-4000, ED-600, ED-900, ED-2003, at least one of MA-223, MA-240, MA-2200, MA-2203ED of Akeli Technology Co., Ltd.

[0043] In a preferred embodiment, the oxalic acid diester is selected from dialkyl oxalate, preferably at least one selected from diethyl oxalate, dimethyl oxalate, dipropyl oxalate, dibutyl oxalate, and diisopropyl oxalate.

[0044] In a preferred embodiment, the small molecule diamine compound is selected from at least one of NH2-R'-NH2, wherein R' is a group containing a rigid six-membered ring.

[0045] Among them, the rigid group R' in the small molecule diamine compound can cooperate with oxamide to form a hard segment. If the preparation process does not use a small molecule diamine compound with a rigid structure, or the small molecule diamine compound is an aliphatic diamine, then the hard segment is completely provided by oxamide. In this way, the hard segment structure is small and the rigidity is also small. It cannot perform "microphase separation" well in the polyether segment-soft segment "softblock" and cannot provide sufficient "cross-linking points".

[0046] In a further preferred embodiment, R' is selected from one of the structures represented by formula (I-1) to formula (I-6), preferably one of the structures represented by formula (I-1) to formula (I-4):

[0047]

[0048] In formula (I-1) to formula (I-4), R1 to R7 are each independently selected from hydrogen, alkyl or aryl, preferably from hydrogen, C1 to C10 alkyl or C6 to C10 aryl, more preferably from hydrogen or C1 to C6 alkyl; R8 to R9 are each independently selected from alkylene or arylene, preferably from C1 to C10 alkylene or C6 to C10 arylene, more preferably from C1 to C6 alkylene.

[0049] Among them, the C1~C10 can be C1, C2, C4, C6, C8 or C10, the C6~C10 can be C6, C7, C8, C9 or C10, and the C1~C6 can be C1, C2, C3, C4, C5 or C6.

[0050] Preferably, R' is selected from one of the following structures:

[0051]

[0052] In a further preferred embodiment, the small molecule diamine compound is selected from at least one of p-phenylenediamine, 2,2-bis(4-aminophenyl)propane, 4,4'-diaminodiphenylmethane, lysine cyclodipeptide (also known as: 6-bis(4-aminobutyl)piperazine-2,5-dione), 4,4'-biphenylenediamine, 1,3-cyclohexanedimethylamine, and 1,4-cyclohexanedimethylamine.

[0053] Among them, the structures of the above-mentioned several small molecule diamine compounds are as follows:

[0054]

[0055] In a preferred embodiment, the preparation method comprises: (1) mixing polyetheramine, oxalic acid and / or oxalic acid diester, and obtaining an oxalic acid amide ester-terminated polyether compound through reaction and post-treatment; (2) reacting the oxalic acid amide ester-terminated polyether compound with a small molecule diamine compound to obtain the polyoxamide. The specific reaction process is as follows:

[0056]

[0057]

[0058] In a preferred embodiment, in step (1), the molar amount of the oxalic acid and / or oxalic acid diester is greater than the molar amount of the polyetheramine.

[0059] In a further preferred embodiment, in step (1), the ratio of the molar amount of the oxalic acid and / or oxalic acid diester to the molar amount of the polyetheramine is greater than or equal to 2:1.

[0060] In a further preferred embodiment, in step (1), the ratio of the molar amount of the oxalic acid and / or oxalic acid diester to the molar amount of the polyetheramine is (3-8):1, preferably (4-6):1, for example, 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1.

[0061] In a preferred embodiment, in step (1), the reaction temperature is 50 to 120° C., and / or the reaction time is 2 to 8 hours, and / or the reaction is carried out at normal pressure.

[0062] For example, the reaction temperature is 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, and / or the reaction time is 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.

[0063] In a preferred embodiment, in step (1), the post-treatment includes: (preferably at 80-100°C, if the reaction temperature is lower than 80°C, it needs to be heated to 80-100°C first) vacuum filtration to remove unreacted oxalic acid and / or oxalic acid diester and other small molecule products (such as alcohol, water, etc.).

[0064] In a further preferred embodiment, in the post-treatment of step (1), the pressure of the reduced pressure filtration is -0.01 to -0.1 MPa, for example, -0.01 MPa, -0.02 MPa, -0.04 MPa, -0.06 MPa, -0.08 MPa or -0.1 MPa.

[0065] In a preferred embodiment, in step (2), the molar ratio of the oxalamide-terminated polyether compound or the polyetheramine to the small molecule diamine compound is 1:(0.9-1.1), for example, 1:0.9, 1:1 or 1:1.1.

[0066] In a preferred embodiment, in step (2), the reaction temperature is 50-120° C. (preferably 50-100° C.), and / or the reaction time is 2-8 hours.

[0067] For example, the reaction temperature is 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, and / or the reaction time is 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.

[0068] Among them, the oxalamide ester-terminated polyether compound has a high proportion of polyether segments in its structure (the oxalamide structure has a low weight ratio) and has a very low melting point, below 100°C. Therefore, when the next step of chain extension with a small molecule diamine compound is carried out, the reaction temperature is also relatively low (preferably not higher than 100°C).

[0069] In a preferred embodiment, in step (2), a vacuum pump can be used to remove small molecule byproducts (such as small molecule methanol, ethanol, isobutanol or butanol, etc.) generated during the reaction.

[0070] In the present invention, polyetheramine, oxalic acid and / or oxalic acid diester, and small molecule diamine compounds are used to prepare the highly elastic polyoxamide. The reaction does not require solvents, does not use diisocyanate compounds such as TDI and MDI, and the entire preparation process does not require high temperature.

[0071] The third object of the present invention is to provide the use of the high elastic polyoxamide described in the first object of the present invention or the high elastic polyoxamide obtained by the preparation method described in the second object of the present invention in elastic fibers.

[0072] In a preferred embodiment, the highly elastic polyoxamide is used to prepare elastic fibers by melt spinning.

[0073] The fiber can be obtained, but is not limited to, as follows: the high elastic polyoxamide is shredded, dried, then heated, melted, and extruded in a screw extrusion spinning machine, and then transported to a spinneret for spinning after extrusion.

[0074] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0075] Compared with the prior art, the present invention has the following beneficial effects:

[0076] (1) In the present invention, the polyoxamide has a soft segment and a hard segment, such as Figure 1 As shown, Represents the soft block, i.e. the polyether segment, represents a hard block, i.e., an oxalamide segment, thus forming a linear structure of soft and hard interlocking, giving the polyoxalamide high elasticity;

[0077] (2) The highly elastic polyoxamide of the present invention has a simple preparation process, a stable source of raw materials, and no highly toxic diisocyanate compounds are used in the production. At the same time, due to the rigidity and polarity of the aromatic diamine dioxamide and cyclic dipeptide diamine dioxamide structures introduced into the main chain of the molecule as the "hard block" of the elastic polyoxamide, the prepared elastic polyoxamide has a high elastic recovery rate when applied to fibers;

[0078] (3) The fiber prepared using the high elastic polyoxamide has high elongation at break, high breaking strength, high 200% stress and excellent elastic recovery (eg 200% elastic recovery). BRIEF DESCRIPTION OF THE DRAWINGS

[0079] Figure 1 Schematic diagram showing the structure of an elastic fiber when stretched or in a solvent;

[0080] Figure 2 A schematic diagram showing the structure of the soft segment and the hard segment in the highly elastic polyoxamide of the present invention;

[0081] Figures 3-4 The DSC graphs of the highly elastic polyoxamide obtained in Examples 1 and 2 are shown respectively;

[0082] Figure 5 A TG chart of the highly elastic polyoxamide obtained in Example 1 is shown. DETAILED DESCRIPTION

[0083] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0084] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0085] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0086] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0087] [Example 1]

[0088] In a dry, anhydrous 5L four-necked flask, add 1417.06g of dimethyl oxalate (12mol, produced by Sinopharm Group), heat to 50°C to melt, quickly add 1800g (2mol, produced by Yangzhou Chenhua New Materials Co., Ltd., molecular weight 900) of polyetheramine CAED900 while stirring, and keep the temperature at 50°C for 8 hours. Raise the temperature to 100°C, reduce the negative pressure to -0.05Mpa, and remove the excess dimethyl oxalate and methanol generated by the reaction. When no more liquid is extracted from the system, the reaction stops, and an oxalamide ester-terminated polyether compound is obtained;

[0089] Add 216.28 g (2 mol) of p-phenylenediamine to the above reaction system, raise the temperature to 100°C, and use a vacuum pump to remove the methanol generated by the reaction. Perform a chain extension reaction for 2 hours to obtain highly elastic polyoxamide. Product No. 1#. GPC test was performed on the product, and the GPC results are as follows:

[0090]

[0091] [Example 2]

[0092] In a dry, anhydrous 10L four-necked flask, add 1315.3g of diethyl oxalate (9mol, produced by Sinopharm Group), heat to 50°C, quickly add 6000g (3mol, produced by Yangzhou Chenhua New Materials Co., Ltd., molecular weight 2000) of polyetheramine CAD2000 while stirring, then heat to 100°C and keep 100°C for reaction for 2 hours, then reduce the negative pressure to -0.1Mpa, and remove the excess diethyl oxalate and ethanol generated by the reaction. When no more liquid is extracted from the system, the reaction stops, and an oxalamide ester-terminated polyether compound is obtained;

[0093] 611.1 g (2.7 mol) of 2,2-bis(4-aminophenyl)propane was added to the above reaction system, and the temperature was raised to 100° C., while ethanol generated by the reaction was evaporated, and a chain extension reaction was carried out for 3 hours to obtain highly elastic polyoxamide.

[0094] Product No. 2#. The product was tested by GPC, and the GPC results are as follows:

[0095]

[0096] [Example 3]

[0097] In a dry, anhydrous 5L four-necked flask, add 2922.8g of diethyl oxalate (20mol, produced by Sinopharm Group), heat to 50°C, quickly add 6000g (10mol, produced by Yangzhou Chenhua New Materials Co., Ltd., molecular weight 600) of polyetheramine CAED600 while stirring, keep the reaction at 50°C for 8 hours, then raise the temperature to 100°C and reduce the negative pressure to -0.1Mpa, and remove the excess diethyl oxalate and ethanol generated by the reaction. When no more liquid is extracted from the system, the reaction stops, and an oxalamide ester-terminated polyether compound is obtained;

[0098] 1981.2 g (10 mol) of 4,4'-diaminodiphenylmethane was added to the above reaction system, and the temperature was raised to 50° C., while ethanol generated by the reaction was evaporated, and the chain extension reaction was carried out for 8 hours to obtain highly elastic polyoxamide.

[0099] Product No. 3#. The product was tested by GPC, and the GPC results are as follows:

[0100]

[0101] [Example 4]

[0102] In a dry, anhydrous 5L four-necked flask, add 857.4g of dimethyl oxalate (7.2mol, produced by Sinopharm Group), heat to 60°C to melt, quickly add 3600g (1.8mol, produced by Yangzhou Chenhua New Materials Co., Ltd., molecular weight 2000) of polyetheramine CAED 2003 while stirring, and keep the temperature at 60°C for 6 hours. Raise the temperature to 100°C, reduce the negative pressure to -0.05Mpa, and remove the excess dimethyl oxalate and methanol generated by the reaction. When no more liquid is extracted from the system, the reaction stops, and an oxalamide ester-terminated polyether compound is obtained;

[0103] Add 297.4 g (1.5 mol) of 4,4'-diaminodiphenylmethane and 76.86 g (0.3 mol, McLean Reagent Company) of lysine cyclodipeptide to the above reaction system, heat to 100°C, evaporate the methanol generated by the reaction, and carry out chain extension reaction for 2 hours to obtain highly elastic polyoxamide. Product No. 4#. GPC test was performed on the product, and the GPC results are as follows:

[0104]

[0105] [Example 5]

[0106] In a dry, anhydrous 10L four-necked flask, add 1096.1g of diethyl oxalate (7.5mol, produced by Sinopharm Group), heat to 50°C, and quickly add 6000g (1.5mol, produced by Huntsman, molecular weight 4000) of polyetheramine while stirring. D 4000, after heating to 90℃ and maintaining 90℃ for 3 hours, the negative pressure is reduced to -0.1Mpa, and the excess diethyl oxalate and ethanol generated by the reaction in the system are pumped out. When no more liquid is pumped out of the system, the reaction stops, and an oxalamide ester-terminated polyetheramine compound is obtained;

[0107] Add 226.15 g (1 mol) of 2,2-bis(4-aminophenyl)propane and 72.12 g (0.364 mol) of 4,4'-diaminodiphenylmethane to the above reaction system, heat to 50°C, evaporate the ethanol generated by the reaction, and perform chain extension reaction for 8 hours to obtain highly elastic polyoxamide. Product No. 5#. GPC test was performed on the product, and the GPC results are as follows:

[0108]

[0109] [Example 6]

[0110] In a dry, anhydrous 10L four-necked flask, add 2630.52g of diethyl oxalate (18mol, produced by Sinopharm Group), heat to 50°C, quickly add 6000g (3mol, produced by Akeli Technology Co., Ltd., molecular weight 2000) of polyetheramine MA-2200 while stirring, heat to 80°C and keep 80°C for 6 hours, then reduce the negative pressure to -0.1Mpa, and remove the excess diethyl oxalate and ethanol generated by the reaction. When no more liquid is extracted from the system, the reaction stops, and an oxalamide ester-terminated polyetheramine compound is obtained;

[0111] 646.12 g (2.857 mol) of 2,2-bis(4-aminophenyl)propane was added to the above reaction system and the temperature was raised to 70°C. The ethanol generated by the reaction was evaporated and the chain extension reaction was carried out for 7 hours to obtain a highly elastic polyoxamide. Product No. 6#. The product was tested by GPC. The GPC results are as follows:

[0112]

[0113] [Comparative Example 1]

[0114] The process of Example 1 was repeated, except that an equal molar amount of ethylenediamine was used to replace p-phenylenediamine, and other conditions remained unchanged.

[0115]

Performance Test 1

[0116] The polyoxamide polymer sample prepared in the embodiment was cut into pieces, dried, and then heated, melted, and extruded in a screw extrusion spinning machine. After extrusion, it was transported to a spinneret for spinning, and the spinning speed was 450m / min; the screw speed was 50r / min, the head temperature during spinning was 220℃, and the screw pressure was 8.6Mpa. The prepared fiber specification was 237dtx / 36f, the draft ratio was 6 times, the draft temperature was 25℃, and the heat setting temperature was 150℃. The performance test standards of the obtained fiber are as follows:

[0117] Elastic recovery rate / %: FZ / T 50007-2012;

[0118] Elongation at break (ELO) / %: FZ / T 50006-2013;

[0119] Breaking strength (TEN) / cN tex-1: FZ / T 50006-2013;

[0120] 200% stress / cN: FZ / T 50006-2013.

[0121] Table 1. Fiber properties test of elastic polymer melt spinning prepared in the examples

[0122] Sample No. TEN(cN) ELO(%) Strength at 200% elongation (cN) 200% elastic recovery rate / % 1# 122.31 200.72 163.4 89.5 2# 126.34 224.73 165.2 92.5 3# 117.63 167.39 182.1 -- 4# 136.47 265.73 154.32 98.3 5# 116.13 304.39 102.35 86.4 6# 143.08 285.06 141.84 98.2 7# 97.21 138.4 87.12 --

[0123] It can be seen from Table 1 that the fibers of the 1~6# elastic polymers prepared in the examples all have good elastic recovery after melt spinning, and the 200% elastic recovery is all above 85% (except for sample 3, because its ELO (%) is only 167%, there is no 200% recovery), and the 200% deformation is all above 100cN.

[0124] However, the elongation at break, breaking strength and 200% stress of the fiber of the 7# elastic polymer prepared in Comparative Example 1 after melt spinning are all lower than those in the examples.

[0125]

Performance Test 2

[0126] The high elastic polyoxamide obtained in Examples 1 and 2 was subjected to DSC testing, and the results were as follows: Figures 3-4 As shown; the high elastic polyoxamide obtained in Example 1 was subjected to TG test, and the results were as follows Figure 5 As shown. Figures 3 to 5 It can be seen that the highly elastic polyoxamide obtained in the present invention has good thermal properties.

[0127] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A highly elastic polyoxamide, the molecular structure of which contains a polyether chain structural unit and an oxamide structural unit represented by formula (I): in, R' is a group containing a rigid six-membered ring.

2. The highly elastic polyoxamide according to claim 1, characterized in that: R' is a group containing a rigid six-membered ring, wherein the rigid six-membered ring is at least one of a cyclohexyl ring, a benzene ring, and a 2,5-diketopiperazine ring; Preferably, R' is selected from one of the structures represented by formula (I-1) to formula (I-6), preferably one of the structures represented by formula (I-1) to formula (I-4): In formula (I-1) to formula (I-4), R1 to R7 are each independently selected from hydrogen, alkyl or aryl, preferably from hydrogen, C1 to C10 alkyl or C6 to C10 aryl, more preferably from hydrogen or C1 to C6 alkyl; R8 to R9 are each independently selected from alkylene or arylene, preferably from C1 to C10 alkylene or C6 to C10 arylene, more preferably from C1 to C6 alkylene.

3. The highly elastic polyoxamide according to claim 1, characterized in that: The molecular structure of the highly elastic polyoxamide contains a repeating structural unit represented by formula (II): In formula (II), R' has the same definition as in formula (I), Represents a polyether chain.

4. The highly elastic polyoxamide according to claim 1, characterized in that: The polyether chain has a molecular weight of 300 to 3000, preferably a molecular weight of 600 to 2000; more preferably, the polyether in the polyether chain is at least one of a homopolymer, a copolymer of two or three of polyoxyethylene, polyoxypropylene and polytetrahydrofuran, for example, at least one of polyoxyethylene, polyoxypropylene, a polyoxyethylene-polyoxypropylene copolymer or polytetrahydrofuran.

5. The highly elastic polyoxamide according to claim 1, characterized in that: The highly elastic polyoxamide is selected from at least one of the polymers represented by the following formula (III): In formula (III), R' has the same definition as in formula (I), Represents a polyether chain.

6. A method for preparing a highly elastic polyoxamide, preferably for preparing the highly elastic polyoxamide according to any one of claims 1 to 5, the method comprising: The raw materials including polyetheramine, oxalic acid and / or oxalic acid diester and small molecular diamine compound are reacted to obtain the product.

7. The preparation method according to claim 6, characterized in that: The molecular weight of the polyetheramine is 300 to 3000, preferably 600 to 2000; preferably, the polyetheramine is a terminal 2-functionality polyetheramine, wherein the polyether is at least one of a homopolymer, a copolymer of two or three of polyoxyethylene, polyoxypropylene and polytetrahydrofuran, for example, at least one of polyoxyethylene, polyoxypropylene, a polyoxyethylene-polyoxypropylene copolymer or polytetrahydrofuran.

8. The preparation method according to claim 6, characterized in that: The oxalic acid diester is selected from dialkyl oxalate, preferably at least one selected from diethyl oxalate, dimethyl oxalate, dipropyl oxalate, dibutyl oxalate, and diisopropyl oxalate.

9. The preparation method according to claim 6, characterized in that: The small molecule diamine compound is selected from at least one of NH2-R'-NH2, wherein R' is a group containing a rigid six-membered ring; Preferably, R' is selected from one of the structures represented by formula (I-1) to formula (I-6), preferably one of the structures represented by formula (I-1) to formula (I-4): In formula (I-1) to formula (I-4), R1 to R7 are each independently selected from hydrogen, alkyl or aryl, preferably hydrogen, C1 to C10 alkyl or C6 to C10 aryl, more preferably hydrogen or C1 to C6 alkyl; R8 to R9 are each independently selected from alkylene or arylene, preferably C1 to C10 alkylene or C6 to C10 arylene, more preferably C1 to C6 alkylene; More preferably, the small molecule diamine compound is at least one selected from p-phenylenediamine, 2,2-bis(4-aminophenyl)propane, 4,4'-diaminodiphenylmethane, lysine cyclodipeptide, 4,4'-biphenylenediamine, 1,3-cyclohexyldimethylamine, and 1,4-cyclohexyldimethylamine.

10. The preparation method according to claim 9, characterized in that: The preparation method comprises: (1) mixing polyetheramine, oxalic acid and / or oxalic acid diester, and obtaining an oxalic acid amide ester-terminated polyether compound through reaction and post-treatment; (2) reacting the oxalic acid amide ester-terminated polyether compound with a small molecular diamine compound to obtain the polyoxamide; Preferably, in step (1), the molar amount of the oxalic acid and / or oxalic acid diester is greater than the molar amount of the polyetheramine, preferably, the ratio of the molar amount of the oxalic acid and / or oxalic acid diester to the molar amount of the polyetheramine is greater than or equal to 2:1; more preferably, the ratio of the molar amount of the oxalic acid and / or oxalic acid diester to the molar amount of the polyetheramine is (3-8):1; Preferably, in step (2), the molar ratio of the oxalic acid amide ester-terminated polyether compound or the polyether amine to the small molecule diamine compound is 1:(0.9-1.1).

11. The preparation method according to claim 10, characterized in that: In step (1), the reaction temperature is 50 to 120° C., and / or the reaction time is 2 to 8 hours; and / or, In step (1), the post-treatment includes: vacuum filtration; and / or, In step (2), the reaction temperature is 50-120° C., and / or the reaction time is 2-8 hours.

12. Use of the highly elastic polyoxamide according to any one of claims 1 to 5 or the highly elastic polyoxamide obtained by the preparation method according to any one of claims 6 to 11 in elastic fibers, preferably, preparing elastic fibers by melt spinning using the highly elastic polyoxamide.

Citation Information

Patent Citations

  • Polyether polyamide elastomer

    CN103403064A

  • Polyether polyamide composition

    CN104583321A

  • Polyoxamide composition and preparation method thereof

    CN105924946A

  • Polyamide and preparation method thereof

    CN107915839A

  • Polyamide hot-melt adhesive capable of being molded by low-pressure injection and preparation method thereof

    CN108148198A