Degradable bismaleimide thermosetting resin material and preparation method thereof

By introducing a hexahydrotriazine ring structure into the bismaleimide structure, a biodegradable bismaleimide thermosetting resin material was prepared, solving the problem of the difficulty in degradation of traditional materials and achieving high-performance biodegradability and mechanical properties, making it suitable for electronic devices and the defense industry.

CN118930851AActive Publication Date: 2024-11-12GUANGXI UNIV FOR NATITIES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411014671.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Traditional bismaleimide thermosetting resin materials are difficult to degrade, leading to difficulties in recycling and serious environmental pollution problems. Furthermore, their high curing temperature and crosslinking density result in poor toughness and low elongation at break.

Method used

A reversible dynamic covalent bond hexahydrotriazine ring structure was introduced into the bismaleimide structure, and a biodegradable bismaleimide thermosetting resin material was prepared by Michael addition reaction of a synthesized triamine monomer with an aromatic diamine.

Benefits of technology

The material achieves biodegradability while maintaining good thermal stability and mechanical properties. Its initial thermal decomposition temperature is 357.7℃, and its tensile strength reaches 39.1-50.1 MPa. The material preparation method is simple and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930851A_ABST
    Figure CN118930851A_ABST
Patent Text Reader

Abstract

The invention discloses a degradable bismaleimide thermosetting resin material and a preparation method thereof, and belongs to the technical field of thermosetting resin materials. The bismaleimide thermosetting resin provided by the invention comprises the following components: 1, 3, 5-tri (4-propionyl thioether aniline) hexahydro-1, 3, 5-triazine, 2, 2 '-bis [4-(4-aminophenoxy phenyl)] propane and bismaleimide, and the bismaleimide thermosetting resin containing a hexahydrotriazine ring structure is prepared through solution polymerization and high-temperature curing. An acid-sensitive hexahydrotriazine ring structure is introduced into a bismaleimide structure, so that the bismaleimide is endowed with degradability. Compared with traditional thermosetting resin, the bismaleimide resin prepared by the method has degradability, the problem of environmental pollution caused by waste thermosetting resin can be solved, and sustainable development is realized at the same time. The thermosetting resin has great application prospects in the aspects of aeronautical materials, electronic devices and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermosetting resin materials, and in particular to a degradable bismaleimide thermosetting resin material containing a hexahydrotriazine ring structure and a preparation method thereof. Technical Background

[0002] Bismaleimide (BMI) is a bifunctional compound with maleimide as the terminal group in its molecular structure. It has excellent heat resistance, flame retardancy and good dielectric properties and is widely used in advanced resin-based composite materials, high temperature resistant insulation materials, flame retardant materials and high temperature adhesives. However, thermosetting bismaleimide resin has good chemical stability and thermal stability due to its own stable irreversible covalent cross-linked network, but it is easy to cause waste of resources and even cause serious environmental pollution problems due to the difficulty of recycling. To solve this problem, a degradable hexahydrotriazine ring structure can be introduced into its structure to give bismaleimide resin degradability.

[0003] In recent years, bismaleimide (BMI) resin has been widely used in various fields such as aerospace, electronic devices, microelectronics, and national defense due to its excellent heat resistance, moisture resistance, corrosion resistance, and good dielectric properties. However, due to the high curing temperature, high crosslinking density, and strong rigidity of the molecular chain of bismaleimide (BMI), it cannot be melted and processed again, has poor toughness, and has low elongation at break. Therefore, it is indispensable to toughen and modify BMI resin while making bismaleimide (BMI) degradable.

[0004] Therefore, in order to fundamentally solve the problem of thermosetting resin degradation, in addition to breaking the three-dimensional cross-linked network of thermosetting resin through harsh chemical conditions, researchers have used another milder chemical degradation method, namely, introducing reversible dynamic covalent bonds into the structure of thermosetting resin. Dynamic covalent bonds include DA bonds, disulfide bonds, disulfide bonds, borate bonds, hexahydrotriazine, imine bonds, acetals, etc., and introducing these structures makes thermosetting resin degradable. Due to the highly cross-linked structure of thermosetting resin materials, this material is difficult to decompose in nature, and discarded thermosetting resins will cause serious environmental pollution problems. Considering these sustainable development issues, future thermosetting resin materials are expected to combine the characteristics of being degradable and environmentally friendly; therefore, it is of great significance to prepare a degradable bismaleimide thermosetting resin material.

[0005] Since the traditional bismaleimide thermosetting resin has the problem of being infusible, its recycling and use is more difficult than that of linear polymer materials. In order to give the material degradable performance and ecological sustainability, the present invention uses a triamine (PTHT) containing an acid-sensitive hexahydrotriazine ring structure to modify the bismaleimide resin. This special structure can be quickly decomposed under acidic conditions, thereby giving the thermosetting bismaleimide resin degradable properties. Summary of the invention

[0006] The present invention aims to provide a degradable bismaleimide thermosetting resin material and a preparation method thereof, and introduces a method of a reversible dynamic covalent bond hexahydrotriazine ring structure into a bismaleimide structure so that the prepared bismaleimide thermosetting resin material has degradability, so as to solve the problems of harsh degradation conditions and difficult recycling of bismaleimide thermosetting resin. The material preparation method is simple, the performance is good, and the material has potential application value in the fields of electronic devices and defense industry.

[0007] In order to achieve the technical objectives of the present invention, the specific technical solution is:

[0008] By synthesizing a triamine monomer and introducing a hexahydrotriazine ring structure, the polymer structure contains a reversible dynamic covalent bond; its heat resistance, degradability and mechanical properties are regulated by the group ratio of the three monomers. The synthetic reaction structure is as follows:

[0009]

[0010] Wherein R is: aromatic diamine.

[0011] The triamine monomer is a monomer containing an acid-sensitive hexahydrotriazine ring structure, and the reaction structure diagram of its synthesis is as follows:

[0012]

[0013] The present invention also provides a method for preparing a degradable bismaleimide thermosetting resin material, comprising the following steps:

[0014] S1. Under a nitrogen atmosphere, a certain amount of bismaleimide was weighed, and then an aromatic diamine was dissolved in an organic solvent and added to the reaction system for Michael addition reaction. The mixture obtained by polymerization reaction at 130° C. for 2 h was the synthesized linear oligomer;

[0015] S2. The linear oligomer of S1 is subjected to a bulk cross-linking reaction. A certain amount of triamine is weighed and dissolved in a solvent, and added to the reaction system to continue the reaction for 1 hour. After the reaction is completed, the reaction liquid is poured into a stainless steel sample mold coated with a release agent for leveling, and placed in an oven for programmed temperature rise. It is high-temperature cured under a temperature rise program of 150℃ / 2h+180℃ / 2h+200℃ / 2h+220℃ / 2h+240℃ / 4h to obtain a degradable bismaleimide thermosetting resin material.

[0016] Furthermore, the bismaleimide is N,N′-(4,4′-methylenediphenyl)bismaleimide.

[0017] Furthermore, the aromatic diamine includes one or more of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl disulfide, 4,4'-diaminodiphenyl sulfide, and 4,4'-diaminodiphenylmethane.

[0018] Furthermore, the triamine includes 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine (PTHT) monomer, which contains an acid-sensitive hexahydrotriazine ring structure, and the NH2 in the structure undergoes Michael addition reaction with the carbon-carbon double bond in bismaleimide.

[0019] Furthermore, the solvent includes one or more of NN-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, and NN-dimethylacetamide.

[0020] Furthermore, the degradable bismaleimide resin can be degraded in an acid-containing solution, and the acid substance includes one or more of nitric acid, sulfuric acid, hydrochloric acid, and phosphoric acid.

[0021] Furthermore, the high temperature curing procedure is 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h.

[0022] Compared with the prior art, the present invention has the following technical advantages:

[0023] (1) The hexahydrotriazine ring structure is introduced into the bismaleimide structure of the present invention, which imparts the thermosetting resin with degradability, and has a very important reference significance for the construction of high-performance degradable thermosetting resin materials.

[0024] (2) The degradable thermosetting resin provided by the present invention has good thermal stability, and the initial thermal decomposition temperature is 357.7°C.

[0025] (3) The degradable bismaleimide thermosetting resin provided by the present invention has good mechanical properties and a tensile strength of 39.1-50.1 MPa.

[0026] (4) The resin material preparation method of the present invention is simple, efficient, and mild in conditions, and bismaleimide resin materials with different properties can be obtained by adjusting the ratio of monomers. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic structural diagram of the bismaleimide of the present invention.

[0028] Figure 2 It is the FTIR spectra of the raw material monomer of the present invention and bismaleimide with different monomer ratios.

[0029] Figure 3 It is the TGA curve diagram of bismaleimide prepared with different group ratios of the present invention.

[0030] Figure 4 It is the DSC curve diagram of bismaleimide prepared with different group ratios of the present invention.

[0031] Figure 5 It is a digital diagram of the degradation of bismaleimide prepared with different group ratios in nitric acid solution. DETAILED DESCRIPTION

[0032] The present invention is further described in detail herein with reference to the following specific embodiments and accompanying drawings, and the present invention is not limited to the following implementation cases. Without departing from the concept and scope of the present invention, the advantages and all changes that can be thought of by the relevant technicians in the field of polymer self-healing materials are included in the present invention, and the present invention covers all modifications, substitutions, equivalent methods and schemes defined by the claims within the concept and scope of the present invention. The preparation process, reaction conditions, reagents, experimental methods, etc. for implementing the present invention, except for the contents specifically involved below, are all common knowledge and common sense in the field, and the present invention has no specific limiting contents. In order to enable the public to better understand the present invention, some specific details are described in detail here. For those skilled in the art, the present invention can be fully understood without these details.

[0033] The reaction flow diagram of the degradable bismaleimide of the present invention is shown in the following figure:

[0034]

[0035] Wherein R is: aromatic diamine.

[0036] The following is further described by means of specific examples.

[0037] The present invention fixes the ratio of maleimide group to amino group at 2:1, and adjusts the ratio of aromatic diamine to triamine to explore the influence on various properties of the material. BMI-BAPP-PTHT-210 / 621 / 411 / 621 / 201 correspond to Examples 1, 2, 3, 4, and 5, respectively, as shown in Table 1.

[0038] Table 1 Design table of material dosage in different group ratios

[0039]

[0040] Example 1

[0041] A method for preparing a degradable bismaleimide thermosetting resin material comprises the following steps:

[0042] (1) Place N,N′-(4,4′-methylenediphenyl)bismaleimide (7.88 g, 22 mmol) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (4.51 g, 11 mmol) in a three-necked flask with a mechanical stirrer, heat to 130°C and stir for 2 h. Use DMF to adjust the viscosity of the system.

[0043] (2) After the reaction is completed, the reaction solution is poured into a stainless steel sample mold coated with a release agent, and then placed in an oven for high-temperature curing at 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h.

[0044] Example 2

[0045] A method for preparing a degradable bismaleimide thermosetting resin material comprises the following steps:

[0046] (1) Place N,N′-(4,4′-methylenediphenyl)bismaleimide (6.62 g, 18.5 mmol) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (2.53 g, 6.16 mmol) in a three-necked flask with a mechanical stirrer, heat to 130°C and stir for 2 h. Use DMF to adjust the viscosity of the system.

[0047] (2) 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine (1.28 g, 2.05 mmol) was dissolved in DMF and added to (1) to continue the reaction. After the reaction was completed, the reaction solution was poured into a stainless steel sample mold coated with a release agent, and then placed in an oven for a procedure including 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h for high temperature curing.

[0048] Example 3

[0049] A method for preparing a degradable bismaleimide thermosetting resin material comprises the following steps:

[0050] (1) Place N,N′-(4,4′-methylenediphenyl)bismaleimide (6.28 g, 17.5 mmol) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (1.80 g, 4.39 mmol) in a three-necked flask with a mechanical stirrer, heat to 130°C and stir for 2 h. Use DMF to adjust the viscosity of the system.

[0051] (2) 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine (1.82 g, 2.91 mmol) was dissolved in DMF and added to (1) to continue the reaction. After the reaction was completed, the reaction solution was poured into a stainless steel sample mold coated with a release agent, and then placed in an oven for a procedure including 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h for high temperature curing.

[0052] Example 4

[0053] A method for preparing a degradable bismaleimide thermosetting resin material comprises the following steps:

[0054] (1) Place N,N′-(4,4′-methylenediphenyl)bismaleimide (5.98 g, 16.7 mmol) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (1.14 g, 2.78 mmol) in a three-necked flask with a mechanical stirrer, heat to 130°C and stir for 2 h. Use DMF to adjust the viscosity of the system.

[0055] (2) 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine (2.31 g, 3.70 mmol) was dissolved in DMF and added to (1) to continue the reaction. After the reaction was completed, the reaction solution was poured into a stainless steel sample mold coated with a release agent, and then placed in an oven for a procedure including 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h for high temperature curing.

[0056] Example 5

[0057] A method for preparing a degradable bismaleimide thermosetting resin material comprises the following steps:

[0058] (1) Place N,N′-(4,4′-methylenediphenyl)bismaleimide (5.37 g, 15 mmol) and 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine (3.12 g, 5 mmol) in a three-necked flask with a mechanical stirrer, heat to 130°C and stir for 2 h. Use DMF to adjust the viscosity of the system.

[0059] After the reaction is completed, the reaction liquid is poured into a stainless steel sample mold coated with a release agent, and then placed in an oven for high-temperature curing at 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h.

[0060] Various performance tests were performed on Examples 1-5, and the results are as follows:

[0061] Table 2 shows the main performance indicators of Examples 1-5

[0062]

[0063] See also Figure 1 The degradable bismaleimide resin prepared in Examples 1-5 has a reversible dynamic covalent hexahydrotriazine ring in its structure. The acid sensitivity of the hexahydrotriazine ring enables the bismaleimide resin to be completely degraded in an acidic environment. The degradation performance, mechanical properties and thermal stability of the bismaleimide resin material can be adjusted by adjusting the ratio of the maleimide group, the aromatic diamine and the amino group in the triamine in the bismaleimide structure.

[0064] See also Figure 2 The figure shows the curing products of BMI, BAPP, PTHT and bismaleimide resin with different group ratios at 4000-600cm -1 FTIR spectrum in the range of BMI at 1142, 828 and 683 cm -1 The absorption bands of maleimide group are shown at 3411-3452 cm-1, which are attributed to the asymmetric stretching vibration of maleimide CNC, out-of-plane bending of =CH and ring deformation. -1 3337-3362cm -1 and 1597-1634cm -1 In the FTIR spectra of all cured products, the absorption bands characteristic of maleimide and primary amine were absent, and a very weak absorption band was caused by the relatively strong asymmetric stretching vibration (CNC) of succinimide, with a band at 1167 cm -1These results indicate that the Michael addition of maleimide groups to primary amines proceeds almost completely at a 2:1 molar ratio of groups.

[0065] See also Figure 3 From the TGA curve, it can be seen that with the increase of PTHT content, the 5% thermal decomposition temperature and the maximum thermal decomposition temperature of BMI resin both decrease. The possible reasons are as follows:

[0066] (1) After adding PTHT, the gel time of the reaction system becomes shorter, resulting in incomplete reaction between the groups. The residue content of the prepared BMI resin increases, affecting the thermal stability of the material.

[0067] (2) The PTHT structure contains unstable structures such as fatty chains. As the proportion of PTHT increases, the content of thermally unstable groups in the polymer increases, resulting in a decrease in the thermal stability of the material.

[0068] See also Figure 4 From the DSC curve, it can be seen that the glass transition temperature of BMI resin is g Between 197.8-221.6℃, when the PTHT content is 0, T g is 207.6℃. With the increase of PTHT content, T g The reason is that with the increase of PTHT content, the crosslinking density increases and the rigidity of the material becomes stronger. However, when the PTHT content accounts for 100% of -NH2 in the system, Tg decreases to 197.8℃. The reason is that PTHT is highly active. After adding more triamine, the gel time of the reaction system becomes shorter. There may be unreacted groups that make the reaction incomplete, which leads to a decrease in the rigidity of the material and Tg decreases. g After the curing process, the BMI resin cured products had no obvious exothermic peaks, indicating that the resins were completely cured. BMI-BAPP-PTHT-201 had an endothermic peak near 200°C, which may be due to the endothermic phenomenon that the bismaleimide cured product experienced a transition from a glassy state to a rubbery state at this temperature.

[0069] See also Figure 5 , the degradation effect diagram of bismaleimide solids with different group ratios in nitric acid aqueous solution, the 210 solidified product without adding PTHT appears in small pieces, and the solid matter in the degradation product becomes less after adding PTHT, and the degradation effect becomes more obvious with the increase of PTHT content, because PTHT contains acid-sensitive hexahydrotriazine ring structure, and the degradation effect becomes more obvious with the increase of its structure content.

[0070] The above contents are further detailed descriptions of the present invention in combination with specific / preferred implementations, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, they can also make several substitutions or modifications to these described embodiments without departing from the concept of the present invention, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention.

Claims

1. A degradable bismaleimide thermosetting resin material, characterized in that: A hexahydrotriazine ring structure is introduced by synthesizing a triamine monomer, so that the polymer structure contains a reversible dynamic covalent bond; its heat resistance, degradability and mechanical properties are regulated by the group ratio of the three monomers. The synthesis reaction structure is as follows: Wherein R is: aromatic diamine.

2. A degradable bismaleimide thermosetting resin material according to claim 1, characterized in that: The triamine monomer is a monomer containing an acid-sensitive hexahydrotriazine ring structure, and the reaction structure diagram of its synthesis is as follows:

3. A method for preparing the degradable bismaleimide thermosetting resin material according to claim 1, characterized in that: The following steps are involved: (1) Under a nitrogen atmosphere, a certain amount of bismaleimide is weighed, and then an aromatic diamine is dissolved in an organic solvent and added to a reaction system to carry out a Michael addition reaction, and a mixture obtained by the reaction is a synthesized linear oligomer; (2) subjecting the linear oligomer of step (1) to a bulk cross-linking reaction, weighing a certain amount of triamine, dissolving it in a solvent, and adding it to the reaction system to continue the reaction; after the reaction is completed, pouring the reaction liquid into a stainless steel sample mold coated with a release agent for leveling, placing it in an oven for programmed temperature rise and high-temperature curing, thereby obtaining a degradable bismaleimide thermosetting resin material.

4. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The bismaleimide described in step (1) is N,N′-(4,4′-methylenediphenyl)bismaleimide.

5. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The aromatic diamine described in step (1) includes one or more of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl disulfide, 4,4'-diaminodiphenyl sulfide, and 4,4'-diaminodiphenylmethane.

6. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The reaction conditions described in step (1) are polymerization reaction at 130° C. for 2 h.

7. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The triamine described in step (2) includes 1,3,5-tris(4-propionylthiophenylamino)hexahydro-1,3,5-triazine monomer.

8. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The solvent described in step (2) includes one or more of NN-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, and NN-dimethylacetamide.

9. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: In step (2), a certain amount of triamine is weighed and dissolved in a solvent, and then added to the reaction system to continue the reaction for 1 hour.

10. A method for preparing a degradable bismaleimide thermosetting resin material as claimed in claim 3, characterized in that: The high temperature curing procedure described in step (2) is 150°C / 2h+180°C / 2h+200°C / 2h+220°C / 2h+240°C / 4h.

Citation Information

Patent Citations

  • Preparation method of bismaleimide prepreg

    CN112500571A

  • Resin composition and metal laminate

    JP2005171106A

  • Aromatic allyl amine thermosetting resin composition

    US5109087A