Cinnamic acid modified polyarylene sulfide and preparation method thereof

Modification of polyphenylene sulfide by cinnamic acid structural monomer solves the problems of complexity and poor polarity of high molecular weight synthesis, achieves molecular weight improvement and viscosity optimization, and enhances the application potential of the material.

CN118930859APending Publication Date: 2024-11-12XIN NING HE KE JI (CHENG DU) YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411252744.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The high molecular weight synthesis process of existing polyphenylene sulfides is complex and has poor structural polarity, which limits its application scenarios, and it is difficult to achieve the increase in molecular weight and viscosity of linear structures.

Method used

The polyphenylene sulfide is modified by using cinnamic acid structural monomer to increase molecular weight through catalytic effect, form high viscosity and low flow polymer, and enhance molecular chain polarity through photosensitive dual polymerization, thereby improving the affinity with other materials. .

Benefits of technology

The improvement of the molecular weight of polyphenylene sulfide, the optimization of viscosity and fluidity, has been successfully achieved, and its binding force and application potential with other materials has been enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032938780000061
    Figure BDA0005032938780000061
  • Figure BDA0005032938780000062
    Figure BDA0005032938780000062
  • Figure BDA0005032938780000071
    Figure BDA0005032938780000071
Patent Text Reader

Abstract

The invention relates to cinnamic acid modified polyarylene sulfide and a preparation method thereof, and belongs to the field of high polymer material synthesis. The preparation method of the cinnamic acid modified polyarylene sulfide comprises the step of carrying out polymerization reaction on a polymeric monomer dihalogenated aromatic compound, dihalogenated cinnamic acid and a sulfur-containing monomer to obtain the cinnamic acid modified polyarylene sulfide, wherein the dihalogenated cinnamic acid is subjected to light treatment before the polymerization reaction or the obtained product is subjected to light treatment after the polymerization reaction so as to induce the photo-dimerization reaction. The cinnamic acid structural monomer is adopted to modify the polyphenylene sulfide structure, and the following effects are achieved: the molecular weight of the polyphenylene sulfide is increased through the catalytic effect of cinnamic acid on the synthesis of the polyphenylene sulfide; through the photosensitive dimerization effect of cinnamic acid, a double-molecular-weight structure is formed, larger molecular weight and molecular structure are formed, and a polymer with high viscosity and low fluidity is obtained; the molecular chain polarity is enhanced by using carboxyl of cinnamic acid, and the affinity and binding force with other materials are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to cinnamic acid-modified polyarylene sulfide and a preparation method thereof, and belongs to the field of polymer material synthesis. Background Art

[0002] Polyarylene sulfide, such as polyphenylene sulfide (PPS), polyphenylene sulfide ketone (PPSK), polyphenylene sulfide sulfone (PPSF), has the characteristics of high temperature resistance, chemical corrosion resistance, excellent electrical properties, radiation resistance, flame retardancy, high mechanical strength, dimensional stability, etc. As coatings, plastics, structural materials, adhesives, fibers and films, they can be widely used in automobiles, aerospace, petrochemicals, light industrial machinery, electronics, food and engineering technology. At present, polyphenylene sulfide can be divided into linear structure, branched structure and cross-linked structure according to its structure. Polyphenylene sulfide with linear structure has the characteristics of high fluidity, low viscosity and high melting point during processing due to its regular molecular chain and high crystallinity. It is widely used in fiber, injection molding and other purposes. Only when the molecular weight reaches a certain level can it be processed into fiber, and resin with higher molecular weight can be used as film raw material. Due to the presence of branches, the regularity of the molecular chain decreases, and the crystallinity decreases, the branched polyphenylene sulfide exhibits a certain toughness, but its melting point varies a lot, and its strength and modulus also vary. It is suitable for applications with higher toughness. Since cross-linked polyphenylene sulfide forms chemical links between molecular chains and multiple molecular weights are linked together, it has a similar body structure. During processing, it has poor fluidity, high viscosity, high strength, and poor toughness. It is used as an injection molded structural part and cannot be used as a fiber. If classified by application scenario, polyphenylene sulfide can be divided into coatings, injection molded parts, fibers, films, and pipes, and the corresponding molecular weights and structures are also different.

[0003] At present, the market is still dominated by linear polyphenylene sulfide resin to increase its molecular weight and reduce its fluidity during processing, increase toughness and strength. However, whether using sodium sulfide process, sodium hydrosulfide process, hydrogen sulfide process or sulfur process, the synthesis of ultra-high molecular weight linear polyphenylene sulfide is a very complicated process, involving additives, purity, pressure, temperature and condition control. On the other hand, even if ultra-high molecular weight polyphenylene sulfide is obtained, its polarity is poor and its inertness is high, and its application scenarios are limited because its structure is composed only of benzene rings and sulfur. Therefore, the modification of the structure of polyphenylene sulfide has never stopped, such as the introduction of sulfone groups, ketone groups, etc. into the main chain, or the introduction of carboxyl groups, hydroxyl groups, etc. into the side groups. However, the increase in molecular weight and viscosity of the linear structure of this type of structure is also a relatively complicated process. New methods and approaches need to be found to increase the molecular weight, reduce the melt index, and enhance the polarity of the molecular chain of linear polyphenylene sulfide. Summary of the invention

[0004] In order to solve the above problems, the present invention uses cinnamic acid structural monomers to modify the structure of polyphenylene sulfide to achieve the following goals: (1) increasing the molecular weight of polyphenylene sulfide through the catalytic effect of cinnamic acid on the synthesis of polyphenylene sulfide; (2) forming a dual molecular weight structure through the photosensitive dimerization effect of cinnamic acid, forming a larger molecular weight and molecular structure, and obtaining a polymer with high viscosity and low fluidity; (3) utilizing the carboxyl group of cinnamic acid to enhance the polarity of the molecular chain, thereby enhancing its affinity and binding force with other materials.

[0005] In order to achieve the above object, the present invention provides a method for preparing a cinnamic acid-modified polyarylene sulfide, which comprises polymerizing a dihalogenated aromatic compound and a dihalogenated cinnamic acid with a sulfur-containing monomer to obtain the cinnamic acid-modified polyarylene sulfide;

[0006] The dihalogenated cinnamic acid is treated with light before the polymerization reaction, or the obtained product is treated with light after the polymerization reaction to induce photodimerization reaction.

[0007] Furthermore, the dihalogenated aromatic compound is selected from p-dihalobenzene 1-Dihalobenzene Naphthalenedihalobenzenes and biphenyl dihalobenzene Dihalogenated quinoline, dihalogenated anthracene, dihalogenated terphenyl, dihalogenated diphenyl ether Dihalobenzophenone Dihalogenated diphenyl sulfone At least one of dihalogenated diphenylmethane, dihalogenated diphenylsilane, dihalogenated diphenylphospholipid, dihalogenated diphenylamide, dihalogenated diphenylimide, dipolyhalogenated pyrrole, dihalogenated furan or dihalogenated thiophene, wherein X=F, Cl or Br.

[0008] Further, the dihalogenated cinnamic acid is selected from trans-2,5-dichlorocinnamic acid (217.05, ), trans-2,4-dichlorocinnamic acid trans-2,6-dichlorocinnamic acid trans-3,4-dichlorocinnamic acid trans-3,5-dichlorocinnamic acid Trans-3,5-difluorocinnamic acid (184.14, ) or trans-2,5-difluorocinnamic acid At least one of .

[0009] Furthermore, the sulfur-containing monomer is selected from sodium sulfide, sodium hydrosulfide and hydrogen sulfide.

[0010] Furthermore, the molar ratio of the dihalogenated aromatic compound to the dihalogenated cinnamic acid is 80-99:1-20.

[0011] Furthermore, the molar ratio of the dihalogenated aromatic compound and the dihalogenated cinnamic acid to the ionic sulfur is 0.99-1.01:1.00.

[0012] Furthermore, the preparation method comprises the following steps: firstly subjecting a sulfur-containing monomer to a dehydration reaction in an organic polar solvent and optionally a base under the protection of an inert gas or nitrogen; then adding a dihalogenated aromatic compound and a dihalogenated cinnamic acid treated with light or not treated with light to react at 200-250° C. for 2-6 hours; then reacting at 250-300° C. for 3-6 hours; then cooling, collecting the synthesized resin, washing, drying, and optionally subjecting the resin to light treatment, to obtain the cinnamic acid-modified polyarylene sulfide.

[0013] Furthermore, the organic polar solvent is selected from at least one of N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide or sulfolane.

[0014] Further, the base comprises NaOH.

[0015] Furthermore, the dehydration reaction is carried out at 150°C to 205°C.

[0016] In some embodiments, if a photo-treated dihalogenated cinnamic acid is added, photo-treatment is not performed after the polymerization is completed, or if a photo-untreated dihalogenated cinnamic acid is added, photo-treatment is performed after the polymerization is completed.

[0017] Furthermore, the light treatment includes using an ultraviolet light source with a wavelength of 300 nm for light treatment.

[0018] Furthermore, the light treatment is performed for 10-30 minutes.

[0019] Furthermore, collecting the synthesized resin includes adding deionized water after cooling, stirring, and filtering to collect the resin.

[0020] Furthermore, the preparation method further comprises extruding and granulating the obtained cinnamic acid-modified polyarylene sulfide.

[0021] Furthermore, the extrusion granulation is carried out using a twin-screw extruder at 300-350°C.

[0022] In other aspects, the present invention provides a cinnamic acid-modified polyarylene sulfide prepared by the method described herein.

[0023] In other aspects, the present invention also provides a cinnamic acid-modified polyarylene sulfide membrane, which is prepared as follows: the cinnamic acid-modified polyarylene sulfide prepared by the method described herein is cast into a cinnamic acid-modified polyarylene sulfide membrane.

[0024] Beneficial effects of the present invention

[0025] As demonstrated in the examples of the present application, the present invention uses cinnamic acid structural monomers to modify the structure of polyphenylene sulfide, and successfully achieves the following goals: (1) increasing the molecular weight of polyphenylene sulfide through the catalytic effect of cinnamic acid on the synthesis of polyphenylene sulfide; (2) forming a dual molecular weight structure through the photosensitive dimerization effect of cinnamic acid, forming a larger molecular weight and molecular structure, and obtaining a polymer with high viscosity and low fluidity; (3) utilizing the carboxyl group of cinnamic acid to enhance the polarity of the molecular chain, thereby enhancing its affinity and binding force with other materials. DETAILED DESCRIPTION

[0026] As a specific example, the present invention uses a dihalogenated cinnamic acid selected from trans-2,5-dichlorocinnamic acid, trans-2,4-dichlorocinnamic acid, trans-2,6-dichlorocinnamic acid, trans-3,4-dichlorocinnamic acid, trans-3,5-dichlorocinnamic acid, trans-3,5-difluorocinnamic acid or trans-2,5-difluorocinnamic acid to modify the structure of polyphenylene sulfide, thereby obtaining a polyphenylene sulfide having a cinnamic acid structure having the following structural formula:

[0027] Schematic structural formula of polyphenylene sulfide containing 2,5-substituted cinnamic acid structure:

[0028] Structure (I):

[0029] Schematic structural formula of polyphenylene sulfide containing 2,4-substituted cinnamic acid structure:

[0030] Structure (II):

[0031] Schematic structural formula of polyphenylene sulfide containing 2,5+2,4 substituted cinnamic acid structure:

[0032] Structure (III):

[0033] Schematic structural formula of polyphenylene sulfide containing 3,5-substituted cinnamic acid structure:

[0034] Structure (IV):

[0035] Wherein, m1 and m2 are the number of monomers of the benzene ring structure, (m1+m2) accounts for 80-99% of the molar number of the molecular chain, and the cinnamic acid monomer accounts for 1-20% of the molar number of the molecular chain.

[0036] Furthermore, the present invention provides a method for preparing cinnamic acid-modified polyarylene sulfide. This technology is further decomposed into (1) halogenated cinnamic acid first forms a dimer under ultraviolet light irradiation, and participates in polymerization reaction in the form of dimer to form a photosensitive polyarylene sulfide containing a cinnamic acid structure. (2) halogenated cinnamic acid first participates in polymerization to form a resin, and then the resin is further subjected to 2+2 reaction of cinnamic acid under ultraviolet light irradiation to form a polyarylene sulfide having a cinnamic acid dimer structure.

[0037] Halogenated cinnamic acid can undergo a 2+2 reaction under ultraviolet irradiation to form a dimer. The present invention uses an ultraviolet light source with a wavelength of 300nm. Halogenated cinnamic acid is dissolved in tetrahydrofuran to form a transparent solution, the joint of the vacuumized cooling pipe is connected and sealed, the bottle body is placed in a water bath and rotated so that the solution is evenly distributed on the bottle wall, the water temperature is increased, and the halogenated cinnamic acid monomer is evenly deposited on the bottle wall, and the cooled tetrahydrofuran is reused; the amount of tetrahydrofuran used to dissolve dihalogenated cinnamic acid is 2.5-10ml of tetrahydrofuran per 1g of monomer. Then a 300nm ultraviolet light source is used to irradiate the bottle wall for 10-30 minutes, and the bottle wall rotates slowly during the irradiation process. After the irradiation is completed, the bottle wall is washed with NMP, and the washing liquid is used for polymerization. Under ultraviolet light, the 2+2 reaction can generally reach 60-90%, not 100% reaction, but regardless of whether the 2+2 reaction occurs, the total molar amount of the halogenated cinnamic acid remains unchanged, so collecting all products (the sum of the products before and after the reaction) to participate in the polymerization reaction can ensure the stability of the total molar ratio of the polymerization reaction. For example, the following dihalogenated cinnamic acid can undergo the following photoreaction:

[0038] (i) Schematic diagram of the formation of trans-2,5-dichlorocinnamic acid dimer:

[0039]

[0040] (ii) Schematic diagram of the formation of trans-2,4-dichlorocinnamic acid dimer:

[0041] (iii) Schematic diagram of the formation of trans-3,5-dichlorocinnamic acid dimer:

[0042] (iv) Schematic diagram of the formation of trans-2,5+2,4-dichlorocinnamic acid dimer:

[0043]

[0044] In the cinnamic acid-modified polyarylene sulfide obtained by polymerizing a dihalogenated aromatic compound and a dihalogenated cinnamic acid with a sulfur-containing monomer, dihalogenated benzene, dihalogenated quinoline, dihalogenated anthracene, dihalogenated terphenyl, dihalogenated diphenyl ether, dihalogenated diphenyl phenone, dihalogenated diphenyl sulfone, dihalogenated diphenyl methane, dihalogenated diphenyl silane, dihalogenated diphenyl phospholipid, dihalogenated diphenyl amide, dihalogenated diphenyl imide, dipolyhalogenated pyrrole, dihalogenated furan or dihalogenated thiophene is used as m1 and m2. More specifically, in the following embodiments, 1,4-dichlorobenzene, 2,4-m-dichlorobenzene, 4,4'-dichlorodiphenyl sulfone, 4,4'-dichlorobenzophenone, etc. are used as main reaction monomers for demonstration;

[0045] Trans-2,5-dichlorocinnamic acid (217.05), trans-2,4-dichlorocinnamic acid, trans-2,6-dichlorocinnamic acid, trans-3,4-dichlorocinnamic acid, trans-3,5-dichlorocinnamic acid, trans-3,5-difluorocinnamic acid (184.14) and trans-2,5-difluorocinnamic acid, as well as the dimer after ultraviolet light irradiation, were used as cinnamic acid monomers for polymerization demonstration;

[0046] The organic polar solvent in the reaction is N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide or cyclopentane sulfone, etc., and the amount of the organic polar solvent is 50-500 ml / mole of polymer monomer (i.e., benzene ring unit + cinnamic acid unit).

[0047] The polymerization reaction is divided into three stages: sodium hydrosulfide activation and dehydration stage, oligomer formation stage and high molecular weight polyarylene sulfide formation stage.

[0048] The purpose of the first stage reaction is to activate sodium hydrosulfide and replace water in sodium hydrosulfide. The specific conditions can be selected by those skilled in the art according to the actual situation. Generally, it can be carried out between 140℃ and 250℃. When the temperature is between 150℃ and 205℃, the effect is better. The second stage is the process of copolymerization of sulfur system and dihalogenated aromatic compound to form uniform oligomers. When the temperature is between 200℃ and 250℃, the effect is best. The third stage is the polymerization reaction to form high molecular weight polyarylene sulfide. When the temperature is between 250℃ and 300℃, the effect is best. The second stage uniformly forms oligomers, and the third stage increases the molecular weight. Each stage contributes differently to the polymerization reaction. The second stage reaction takes 2 to 6 hours, the third stage takes 3 to 6 hours, and the total reaction takes 5 to 12 hours.

[0049] The polymerization is carried out at 200-250° C. for 2-6 hours, then at 250-300° C. for 3-6 hours, and then the temperature is lowered to 150° C. or below to complete the polymerization, and the polyphenylene sulfide containing a cinnamic acid structure is transferred to deionized water, stirred, filtered to remove soluble ions such as soluble sodium chloride, washed with deionized water for 6-9 times, and dried at 80-120° C. for 12-20 hours to obtain the polyphenylene sulfide containing a cinnamic acid structure.

[0050] The invention forms a dual molecular weight structure through the photosensitive dimerization effect of cinnamic acid to form a larger molecular weight and molecular structure, thereby obtaining a polymer with high viscosity and low fluidity; and utilizes the carboxyl group of cinnamic acid to enhance the polarity of the molecular chain, thereby enhancing the affinity and binding force with other materials.

[0051] The third technology provided by the present invention is a further processing technology for polyphenylene sulfide containing cinnamic acid structural elements. The above-mentioned polyphenylene sulfide resin particles containing cinnamic acid structure are vacuum dried at a drying temperature of 80-120°C, and then irradiated under ultraviolet light with a wavelength of 300nm for 10-30 minutes, and extruded and granulated at 300-350°C by a twin-screw extruder to form polyphenylene sulfide pellets containing cinnamic acid structural monomers. An injection molding machine is used to injection mold mechanical specimens at 310-350°C for testing. The above-mentioned polyphenylene sulfide containing cinnamic acid structural monomers is drawn into a film by a casting machine, and the temperature of the first to fourth sections of the screw is 300-350°C, and the speed of the film collection roller is 10 to 300mm / min. Through the casting process, a cast film with a thickness of 10-250μm is formed, and its hydrophilic angle is tested.

[0052] Performance Test:

[0053] Molecular weight and viscosity: expressed by melt index, tested at 315°C and 5kg pressure, the mass in grams flowing out in 10 minutes; g / 10min.

[0054] Film thickness: Labthink CHY-C2A thickness gauge.

[0055] Polyarylene sulfide: Polarity-water contact angle:

[0056] The sample was made into a 2×2 cm film for water contact angle test. The test conditions were as follows: the test temperature was room temperature, the sessile drop method, the drop volume was 2 μL, and six parallel points were measured for each film sample. The statistical analysis software was OriginPro2022b, all data were expressed as mean ± standard deviation, the normality test was performed using the Kolmogorov-Smirnov method, the variance homogeneity test was performed using the Levene method, and the mean comparison was performed using the Scheffe test in One Way ANOVA.

[0057] Melting point: The DSC test was performed using a DSC 3+ differential scanning calorimeter from Mettler-Toledo, Switzerland. Under a nitrogen atmosphere, the sample was first heated from 40°C to 320°C at a heating rate of 10°C / min, maintained at 320°C for 5 min to eliminate the thermal history, then cooled to 40°C at a cooling rate of 10°C / min, and then heated to 320°C at a heating rate of 10°C / min.

[0058] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ): mass to volume ratio, routine test.

[0059] Mechanical properties test: conventional mechanical test

[0060] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0061] Example 1

[0062] (1) Preparation of 2,5-dichlorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 2,5-dichlorocinnamic acid: Dissolve 1085g of 2,5-dichlorocinnamic acid in tetrahydrofuran in a 5L volumetric flask to form a transparent solution. Connect the joint of the vacuum cooling tube and seal it. Place the bottle in a water bath and rotate it so that the solution is evenly distributed on the bottle wall. Increase the water temperature and evacuate the bottle so that the halogenated cinnamic acid monomer is evenly deposited on the bottle wall. The cooled tetrahydrofuran is reused. Then use a 300nm ultraviolet light source to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield rotates slowly so that all monomers can receive uniform ultraviolet light irradiation. After irradiation, use 2L of NMP to wash the bottle wall four times. The washing liquid contains all the added dichlorocinnamic acid (mostly 2,5-dichlorocinnamic acid dimer And a small number of single molecules that did not form dimers ) for the next polymerization reaction.

[0063] (2) Preparation of polyarylene sulfide: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.5kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was distilled out, 13.9kg p-dichlorobenzene was added, 2L 2,5-dichlorocinnamic acid units prepared in (1) were all introduced into the reactor, and 1L NMP was used to wash the volumetric flask twice and added to the reactor. The temperature was gradually raised to 250°C, and the reaction was carried out at this temperature for 3 hours, and the first stage of the reaction was completed; the temperature was raised to 260°C and the reaction was carried out for 3 hours, and the temperature was cooled to 150°C and deionized water was slowly added, filtered, washed once and filtered again, the first filtrate and the second filtrate were combined, and the combined filtrate was sent to a distillation tower to separate water and NMP, and the by-product sodium chloride was collected. The resin was washed with deionized water at 60°C for 6 times. Then it was vacuum dried at 120°C for 24 hours; 10.2kg of white granular polyarylene sulfide product was obtained.

[0064] (3) Granulation of polyarylene sulfide containing cinnamic acid structure: Granulation was performed by extrusion at 300-350°C using a twin-screw extruder, with the first stage temperature at 310°C, the second stage temperature at 325°C, the third stage temperature at 325°C, and the fourth stage temperature at 320°C. The extrusion speed was 25 kg / h. Mechanical specimens were injection molded at 310-350°C using an injection molding machine for testing.

[0065] (4) Film drawing of polyphenylene sulfide with cinnamic acid structure: The polyphenylene sulfide containing cinnamic acid structure monomer of the above (2) was drawn into a film by a casting machine, the temperatures of the first to fourth sections of the screw were 310°C, 325°C, 325°C and 315°C, and the speed of the film collection roller was 10-300 mm / min. During the casting process, the roller speed and tension were controlled to form cast films with two thicknesses of 10 and 250 μm, and their hydrophilic angle and other properties were tested.

[0066] (5) Performance parameter test:

[0067] (i) Product melt index (g / 10min): 180

[0068] (ii) Hydrophilic angle (°): 66

[0069] (iii) Tensile strength (MPa): 75; Flexural strength (MPa): 105 Modulus (GPa): 4.0

[0070] (iv) Melting point (DSC test, heating rate 2°C / min): 286

[0071] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0072] Example 2 (same as Example 1, using 2,4-dichlorocinnamic acid instead of 2,5-dichlorocinnamic acid)

[0073] (1) Preparation of 2,4-dichlorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 2,4-dichlorocinnamic acid: Dissolve 1085g of 2,5-dichlorocinnamic acid in tetrahydrofuran in a 5L volumetric flask to form a transparent solution. Connect the joint of the vacuum cooling tube and seal it. Place the bottle in a water bath and rotate it so that the solution is evenly distributed on the bottle wall. Increase the water temperature and evacuate the bottle so that the halogenated cinnamic acid monomer is evenly deposited on the bottle wall. The cooled tetrahydrofuran is reused. Then use a 300nm ultraviolet light source to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield rotates slowly so that all monomers can receive uniform ultraviolet light irradiation. After irradiation, use 2L of NMP to wash the bottle wall four times. The washing liquid contains all the added dichlorocinnamic acid (mostly 2,4-dichlorocinnamic acid dimer and a small amount of single-molecule 2,4-dichlorocinnamic acid that did not form a dimer ) for the next polymerization reaction.

[0074] (2)-(4) are the same as in Example 1.

[0075] Test results:

[0076] (i) Product melt index (g / 10min): 160

[0077] (ii) Hydrophilic angle (°): 65

[0078] (iii) Tensile strength (MPa): 72; Flexural strength (MPa): 100 Modulus (GPa): 4.0

[0079] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0080] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0081] Example 3 (same as Example 1, using 3,5-dichlorocinnamic acid instead of 2,5-dichlorocinnamic acid)

[0082] (1) Preparation of 3,5-dichlorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 3,5-dichlorocinnamic acid: Dissolve 1085g 3,5-dichlorocinnamic acid in tetrahydrofuran in a 5L volumetric flask to form a transparent solution. Connect the joint of the vacuum cooling tube and seal it. Place the bottle in a water bath and rotate it so that the solution is evenly distributed on the bottle wall. Increase the water temperature and evacuate the bottle so that the halogenated cinnamic acid monomer is evenly deposited on the bottle wall. The cooled tetrahydrofuran is reused. Then use a 300nm ultraviolet light source to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield rotates slowly so that all monomers can receive uniform ultraviolet light irradiation. After irradiation, use 2L of NMP to wash the bottle wall four times. The washing liquid contains all the added dichlorocinnamic acid (mostly 3,5-dichlorocinnamic acid dimer And a small number of single molecules that did not form dimers ) for the next polymerization reaction.

[0083] (2)-(4) are the same as in Example 1.

[0084] Test results:

[0085] (i) Product melt index (g / 10min): 150

[0086] (ii) Hydrophilic angle (°): 66

[0087] (iii) Tensile strength (MPa): 75; Flexural strength (MPa): 105 Modulus (GPa): 4.0

[0088] (iv) Melting point (DSC test, heating rate 2°C / min): 286

[0089] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0090] Example 4 (same as Example 1, except that the single 2,5-dichlorocinnamic acid unit is replaced by trans-2,5+2,4-dichlorocinnamic acid dimer)

[0091] (1) Preparation of trans-2,5+2,4-dichlorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 2,5-dichlorocinnamic acid: 545 g of 2,5-dichlorocinnamic acid and 540 g of 2,4-dichlorocinnamic acid were dissolved in tetrahydrofuran in a 5 L volumetric flask to form a transparent solution. The joint of the vacuum cooling tube was connected and sealed. The bottle was placed in a water bath and rotated to make the solution evenly distributed on the bottle wall. The water temperature was increased and the vacuum was drawn to make the halogenated cinnamic acid monomer evenly deposited on the bottle wall. The cooled tetrahydrofuran was reused. Then, a 300 nm ultraviolet light source was used to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield was rotated slowly so that all monomers could receive uniform ultraviolet light irradiation. After the irradiation was completed, the bottle wall was washed four times with 2 L of NMP. The washing liquid contained all the dichlorocinnamic acid added (mostly trans-2,5+2,4-dichlorocinnamic acid dimer). and a small amount of single-molecule 2,5-dichlorocinnamic acid that did not form a dimer and 2,4-dichlorocinnamic acid ) for the next polymerization reaction.

[0092] (2)-(4) are the same as in Example 1.

[0093] Test results:

[0094] (i) Product melt index (g / 10min): 170

[0095] (ii) Hydrophilic angle (°): 66

[0096] (iii) Tensile strength (MPa): 73; Flexural strength (MPa): 102 Modulus (GPa): 4.0

[0097] (iv) Melting point (DSC test, heating rate 2°C / min): 286

[0098] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0099] Example 5 (same as Example 1, except that the dihalogen cinnamic acid monomer is replaced with 3,5-difluorocinnamic acid)

[0100] (1) Preparation of trans-3,5-difluorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 3,5-trifluorocinnamic acid: 920g 3,5-trifluorocinnamic acid was dissolved in a 5L volumetric flask in tetrahydrofuran to form a transparent solution. The joint of the vacuum cooling tube was connected and sealed. The bottle was placed in a water bath and rotated to make the solution evenly distributed on the bottle wall. The water temperature was increased and the vacuum was drawn to make the halogenated cinnamic acid monomer evenly deposited on the bottle wall. The cooled tetrahydrofuran was reused. Then, a 300nm ultraviolet light source was used to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield was rotated slowly so that all monomers could receive uniform ultraviolet light irradiation. After the irradiation was completed, the bottle wall was washed four times with 2L of NMP. The washing liquid contained all the added dichlorocinnamic acid (mostly trans-3,5-difluorocinnamic acid dimer and a small amount of single-molecule 3,5-difluorocinnamic acid that did not form dimers ) for the next polymerization reaction.

[0101] (2)-(4) are the same as in Example 1.

[0102] Test results:

[0103] (i) Product melt index (g / 10min): 120

[0104] (ii) Hydrophilic angle (°): 67

[0105] (iii) Tensile strength (MPa): 76; Flexural strength (MPa): 106 Modulus (GPa): 4.0

[0106] (iv) Melting point (DSC test, heating rate 2°C / min): 286

[0107] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0108] Example 6 (same as Example 1, but with different 2,5-dichlorocinnamic acid unit contents)

[0109] (1) Same as Example 1

[0110] (2) Preparation of polyarylene sulfide: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.5kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was distilled out, 13.9kg p-dichlorobenzene was added, half of the 2L 2,5-dichlorocinnamic acid unit prepared in (1) (containing a total monomer of 543g) was added to the reactor, and 1L NMP was used to wash the volumetric flask twice and added to the reactor. The temperature was gradually raised to 250°C, and the reaction was carried out at this temperature for 3 hours, and the first stage of the reaction was completed; the temperature was raised to 260°C and the reaction was carried out for 3 hours, and the temperature was cooled to 150°C and deionized water was slowly added, filtered, washed once and filtered again, the first filtrate and the second filtrate were combined, and the combined filtrate was sent to a distillation tower to separate water and NMP, and the by-product sodium chloride was collected. The resin was washed 6 times with deionized water at 60°C. The mixture was then vacuum dried at 120° C. for 24 hours to obtain 10.2 kg of white granular polyarylene sulfide product.

[0111] (3)-(4) Same as Example 1.

[0112] Test results:

[0113] (i) Product melt index (g / 10min): 220

[0114] (ii) Hydrophilic angle (°): 76

[0115] (iii) Tensile strength (MPa): 70; Flexural strength (MPa): 98 Modulus (GPa): 4.0

[0116] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0117] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0118] Example 7 (same as Example 1, but with different content of 2,5-dichlorocinnamic acid units)

[0119] (1) Preparation of 2,5-dichlorocinnamic acid dimer by 2+2 ultraviolet addition reaction of 2,5-dichlorocinnamic acid: 1628g of 2,5-dichlorocinnamic acid was dissolved in tetrahydrofuran in a 10L volumetric flask to form a transparent solution. The joint of the vacuum cooling tube was connected and sealed. The bottle was placed in a water bath and rotated to make the solution evenly distributed on the bottle wall. The water temperature was increased and the vacuum was drawn to make the halogenated cinnamic acid monomer evenly deposited on the bottle wall. The cooled tetrahydrofuran was reused. Then, a 300nm ultraviolet light source was used to irradiate the bottle wall for 15 minutes. During the irradiation process, the shield was rotated slowly so that all monomers could receive uniform ultraviolet light irradiation. After the irradiation was completed, the bottle wall was washed four times with 4L of NMP. The washing liquid contained all the dichlorocinnamic acid added (mostly 2,5-dichlorocinnamic acid dimer). And a small number of single molecules that did not form dimers ) for the next polymerization reaction.

[0120] (2) Preparation of polyarylene sulfide: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.5kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was distilled out, 13.6kg p-dichlorobenzene was added, and all the 2,5-dichlorocinnamic acid units prepared in (1) were introduced into the reactor, and 2L NMP was used to wash the volumetric flask twice and added to the reactor. The temperature was gradually raised to 250°C, and the reaction was carried out at this temperature for 3 hours, and the first stage of the reaction was completed; the temperature was raised to 260°C and the reaction was carried out for 3 hours, and the temperature was cooled to 150°C and deionized water was slowly added, filtered, washed once and filtered again, the first filtrate and the second filtrate were combined, and the combined filtrate was sent to a distillation tower to separate water and NMP, and the by-product sodium chloride was collected. The resin was washed with deionized water at 60°C for 6 times. Then it was vacuum dried at 120°C for 24 hours; 10.3kg of white granular polyarylene sulfide product was obtained.

[0121] (3)-(4) Same as Example 1.

[0122] Test results:

[0123] (i) Product melt index (g / 10min): 110

[0124] (ii) Hydrophilic angle (°): 60

[0125] (iii) Tensile strength (MPa): 78; Flexural strength (MPa): 110 Modulus (GPa): 4.0

[0126] (iv) Melting point (DSC test, heating rate 2°C / min): 288

[0127] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0128] Example 8 (same as Example 1, directly using 2,5-dichlorocinnamic acid to polymerize and then treating the resin with UV light)

[0129] (1) Preparation of polyarylene sulfide: Add 50L NMP into a 100L reactor, remove 11.6kg sodium hydrosulfide (48%) and 4.5kg NaOH under nitrogen protection, heat to 200℃ under nitrogen protection, distill 6.0L water, add 13.9kg p-dichlorobenzene and 1085g 2,5-dichlorocinnamic acid into the reactor. Gradually heat to 250℃, react at this temperature for 3 hours, and the first stage reaction is completed; heat to 260℃ and react for 3 hours, cool to 150℃ and slowly add deionized water, filter, wash once and filter again, combine the first filtrate and the second filtrate, send the combined filtrate to the distillation tower to separate water and NMP, and collect the by-product sodium chloride. The resin is washed with deionized water at 60℃ for 6 times. Then vacuum dry at 120℃ for 24 hours; obtain 10.2kg of white granular polyarylene sulfide product.

[0130] (2) Granulation of polyarylene sulfide containing cinnamic acid structure: The white granular polyarylene sulfide product obtained in (1) was placed in a rotating glass container, and irradiated with ultraviolet light of a wavelength of 300 nm for 30 minutes during the rotation process, and the rotation speed was 60 rpm. Granulation was performed by extrusion at 300-350°C using a twin-screw extruder, with the first section temperature being 310°C, the second section temperature being 325°C, the third section temperature being 325°C, and the fourth section temperature being 320°C. The extrusion speed was 25 kg / h. Mechanical specimens were injection molded using an injection molding machine at 310-350°C for testing.

[0131] (3) The polyphenylene sulfide containing cinnamic acid structure monomer is drawn into a film by a casting machine, the temperatures of the first to fourth sections of the screw are 310° C., 325° C., 325° C. and 315° C., and the speed of the film collection roller is 10 to 300 mm / min. During the casting process, the roller speed and tension are controlled to form two thicknesses of 10 and 250 μm cast films, and their hydrophilic angle and other properties are tested.

[0132] Performance parameter test:

[0133] Test results:

[0134] (i) Product melt index (g / 10min): 180

[0135] (ii) Hydrophilic angle (°): 66

[0136] (iii) Tensile strength (MPa): 73; Flexural strength (MPa): 102 Modulus (GPa): 4.0

[0137] (iv) Melting point (DSC test, heating rate 2°C / min): 287

[0138] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0139] Example 9 (same as Example 5, using 2,5-difluorocinnamic acid instead of 2,5-difluorocinnamic acid, directly using 2,5-difluorocinnamic acid to polymerize and then treating the resin with UV light)

[0140] (1) Preparation of polyarylene sulfide: Add 50L NMP into a 100L reactor, remove 11.6kg sodium hydrosulfide (48%) and 4.5kg NaOH under nitrogen protection, heat to 200℃ under nitrogen protection, distill 6.0L water, add 13.9kg p-dichlorobenzene and 920g 2,5-dichlorocinnamic acid into the reactor. Gradually heat to 250℃, react at this temperature for 3 hours, and the first stage reaction is completed; heat to 260℃ and react for 3 hours, cool to 150℃ and slowly add deionized water, filter, wash once and filter again, combine the first filtrate and the second filtrate, send the combined filtrate to the distillation tower to separate water and NMP, and collect the by-product sodium chloride. The resin is washed with deionized water at 60℃ for 6 times. Then vacuum dry at 120℃ for 24 hours; obtain 10.2kg of white granular polyarylene sulfide product.

[0141] (2)-(4) are the same as Example 9.

[0142] Test results:

[0143] (i) Product melt index (g / 10min): 150

[0144] (ii) Hydrophilic angle (°): 66

[0145] (iii) Tensile strength (MPa): 75; Flexural strength (MPa): 108 Modulus (GPa): 4.0

[0146] (iv) Melting point (DSC test, heating rate 2°C / min): 286

[0147] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0148] Example 10 (same as Example 1, with 4,4-dichlorodiphenyl sulfone added to the benzene ring unit)

[0149] (1) Same as Example 1.

[0150] (2) Preparation of polyarylene sulfide: 50 L NMP, 11.6 kg sodium hydrosulfide (48%), and 4.5 kg NaOH were added to a 100 L reactor, heated to 200 ° C under nitrogen protection, 6.0 L of water was distilled out, 13.2 kg p-dichlorobenzene and 1.44 kg 4-dichlorodiphenyl sulfone were added. All 2L of 2,5-dichlorocinnamic acid units prepared in (1) were introduced into the reactor, and 1L of NMP was used to wash the volumetric flask twice and added to the reactor. The temperature was gradually raised to 250°C, and the reaction was carried out at this temperature for 3 hours. The first stage of the reaction was completed; the temperature was raised to 260°C for reaction for 3 hours, and deionized water was slowly added to 150°C, filtered, washed once and filtered again, and the first filtrate and the second filtrate were combined. The combined filtrate was sent to a distillation tower to separate water and NMP, and the by-product sodium chloride was collected. The resin was washed 6 times with deionized water at 60°C. Then it was vacuum dried at 120°C for 24 hours; 10.5kg of white granular polyarylene sulfide product was obtained.

[0151] (3)-(5) are the same as in Example 1.

[0152] Test results:

[0153] (i) Product melt index (g / 10min): 175

[0154] (ii) Hydrophilic angle (°): 63

[0155] (iii) Tensile strength (MPa): 71; Flexural strength (MPa): 101 Modulus (GPa): 3.9

[0156] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0157] (v) Cast film UV light corresponding wavelength (nm): 300-350

[0158] Comparative Example 1 (general purpose polyphenylene sulfide)

[0159] Add 50L NMP to a 100L reactor, remove 11.6kg sodium hydrosulfide (48%) and 4.5kg NaOH under nitrogen protection, heat to 200℃ under nitrogen protection, distill 6.0L water, and add 14.7kg p-dichlorobenzene. Gradually heat to 250℃, react at this temperature for 3 hours, and the first stage of reaction is completed; heat to 260℃ and react for 3 hours, cool to 150℃ and slowly add deionized water, filter, wash once and filter again, combine the first filtrate and the second filtrate, send the combined filtrate to the distillation tower to separate water and NMP, and collect the by-product sodium chloride. The resin is washed 6 times with deionized water at 60℃. Then vacuum dry at 120℃ for 24 hours; 10.1kg of white granular polyphenylene sulfide product is obtained.

[0160] Test results: The resin melt index is high and cast film is difficult.

[0161] (i) Product melt index (g / 10min): 580

[0162] (ii) Hydrophilic angle (°): 110

[0163] (iii) Tensile strength (MPa): 65; Flexural strength (MPa): 90 Modulus (GPa): 3.9

[0164] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0165] (v) Resin external light corresponding wavelength (nm): not obvious

[0166] Comparative Example 2 (same as Comparative Example 1, 1,4-p-dichlorobenzene was irradiated with 300 nm ultraviolet light for 30 minutes before polymerization)

[0167] Add 50L NMP to a 100L reactor, remove 11.6kg sodium hydrosulfide (48%) and 4.5kg NaOH under nitrogen protection, heat to 200℃ under nitrogen protection, distill 6.0L water, add 14.7kg p-dichlorobenzene irradiated with ultraviolet light for 30 minutes. Gradually heat to 250℃, react at this temperature for 3 hours, and the first stage of the reaction is completed; heat to 260℃ and react for 3 hours, cool to 150℃ and slowly add deionized water, filter, wash once and filter again, combine the first filtrate and the second filtrate, send the combined filtrate to the distillation tower to separate water and NMP, and collect the by-product sodium chloride. The resin is washed 6 times with deionized water at 60℃. Then vacuum dry at 120℃ for 24 hours; 10.1kg of white granular polyphenylene sulfide product is obtained.

[0168] Test results: The resin melt index is high and the cast film is difficult.

[0169] (i) Product melt index (g / 10min): 610

[0170] (ii) Hydrophilic angle (°): 110

[0171] (iii) Tensile strength (MPa): 68; Flexural strength (MPa): 92 Modulus (GPa): 3.9

[0172] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0173] (v) UV light wavelength of resin (nm): not obvious

[0174] Comparative Example 3 (same as Example 10, 4,4-dichlorodiphenyl sulfone was introduced into the benzene ring component, and the 2,5-dichlorocinnamic acid component was removed)

[0175] Add 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.5kg NaOH into a 100L reactor, heat to 200℃ under nitrogen protection, distill out 6.0L water, add 13.95kg p-dichlorobenzene and 1.44kg 4,4-dichlorodiphenyl sulfone. The temperature was gradually raised to 250°C, and the reaction was carried out at this temperature for 3 hours, and the first stage of the reaction was completed; the temperature was raised to 260°C for 3 hours, and the reaction was cooled to 150°C, and deionized water was slowly added, filtered, washed once, and filtered again, and the first filtrate and the second filtrate were combined, and the combined filtrate was sent to a distillation tower to separate water and NMP, and the by-product sodium chloride was collected. The resin was washed with deionized water at 60°C for 6 times. Then it was vacuum dried at 120°C for 24 hours; 10.5 kg of white granular polyarylene sulfide product was obtained.

[0176] Test results: The resin melt index is high and cast film is difficult.

[0177] (i) Product melt index (g / 10min): 520

[0178] (ii) Hydrophilic angle (°): 106

[0179] (iii) Tensile strength (MPa): 68; Flexural strength (MPa): 93 Modulus (GPa): 3.9

[0180] (iv) Melting point (DSC test, heating rate 2°C / min): 285

[0181] (v) UV light wavelength of resin (nm): not obvious

[0182] Comparative Example 4 (same as Comparative Example 3, 4,4-dichlorodiphenyl sulfone was irradiated with 300nm ultraviolet light 30 minutes)

[0183] 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.5kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was distilled out, 13.95kg p-dichlorobenzene and 4,4-dichlorodiphenyl sulfone were added and irradiated with 300nm ultraviolet light for 30 minutes. 1.44kg. Gradually heat to 250℃, react at this temperature for 3 hours, and the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, wash once and filter again, combine the first filtrate and the second filtrate, send the combined filtrate to the distillation tower to separate water and NMP, and collect the by-product sodium chloride. The resin is washed 6 times with deionized water at 60℃. Then vacuum dry at 120℃ for 24 hours; 10.5kg of white granular polyarylene sulfide product is obtained.

[0184] Test results: The resin melt index is high and cast film is difficult.

[0185] (i) Product melt index (g / 10min): 630

[0186] (ii) Hydrophilic angle (°): 106

[0187] (iii) Tensile strength (MPa): 66; Flexural strength (MPa): 95 Modulus (GPa): 3.9

[0188] (iv) Melting point (DSC test, heating rate 2°C / min): 283

[0189] (v) UV light wavelength of resin (nm): not obvious

[0190] Comparative Example 5 (same as Comparative Example 1, irradiating the general polyphenylene sulfide resin with 300 nm ultraviolet light for 30 minutes before extrusion granulation)

[0191] (1) Same as Comparative Example 1

[0192] (2) The white granular polyphenylene sulfide product obtained in Comparative Example 1 was placed in a rotating glass container, and irradiated with ultraviolet light of a wavelength of 300 nm for 30 minutes during the rotation process, and the rotation speed was 60 rpm. The product was extruded and granulated at 300-350°C by a twin-screw extruder, with the first section temperature of 310°C, the second section temperature of 325°C, the third section temperature of 325°C, and the fourth section temperature of 320°C. The extrusion speed was 25 kg / h. Mechanical specimens were injection molded at 310-350°C using an injection molding machine for testing.

[0193] Test results: The resin melt index is high and cast film is difficult.

[0194] (i) Product melt index (g / 10min): 580

[0195] (ii) Hydrophilic angle (°): 110

[0196] (iii) Tensile strength (MPa): 66; Flexural strength (MPa): 92 Modulus (GPa): 3.9

[0197] (iv) Melting point (DSC test, heating rate 2°C / min): 283

[0198] (v) UV light wavelength of resin (nm): not obvious

[0199] It should be noted that the preferred embodiments of the present invention are given in the specification of the present invention, but the present invention can be implemented in many different forms and is not limited to the embodiments described in this specification. These embodiments are not intended to be additional limitations on the content of the present invention. The purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. In addition, the above-mentioned technical features continue to be combined with each other to form various embodiments not listed above, which are all considered to be within the scope of the present invention specification; further, for ordinary technicians in this field, they can be improved or transformed according to the above description, and all these improvements and transformations should belong to the protection scope of the claims attached to the present invention.

Claims

1. A method for preparing cinnamic acid-modified polyarylene sulfide, characterized in that: The method comprises subjecting a polymerizable monomer of a dihalogenated aromatic compound and a dihalogenated cinnamic acid to a polymerization reaction with a sulfur-containing monomer to obtain the cinnamic acid-modified polyarylene sulfide; The dihalogenated cinnamic acid is treated with light before the polymerization reaction, or the obtained product is treated with light after the polymerization reaction to induce photodimerization reaction.

2. The preparation method according to claim 1, characterized in that: The dihalogenated aromatic compound is selected from at least one of p-dihalobenzene, m-dihalobenzene, naphthalenedihalobenzene, biphenyldihalobenzene, dihalogenated quinoline, dihalogenated anthracene, dihalogenated terphenyl, dihalogenated diphenyl ether, dihalogenated diphenyl phenone, dihalogenated diphenyl sulfone, dihalogenated diphenyl methane, dihalogenated diphenyl silane, dihalogenated diphenyl phospholipid, dihalogenated diphenyl amide, dihalogenated diphenyl imide, dipolyhalogenated pyrrole, dihalogenated furan or dihalogenated thiophene.

3. The preparation method according to claim 1, characterized in that: The dihalogenated cinnamic acid is selected from at least one of trans-2,5-dichlorocinnamic acid, trans-2,4-dichlorocinnamic acid, trans-2,6-dichlorocinnamic acid, trans-3,4-dichlorocinnamic acid, trans-3,5-dichlorocinnamic acid, trans-3,5-difluorocinnamic acid and trans-2,5-difluorocinnamic acid.

4. The preparation method according to claim 1, characterized in that: The sulfur-containing monomer is selected from sodium sulfide, sodium hydrosulfide and hydrogen sulfide.

5. The preparation method according to claim 1, characterized in that: The molar ratio of the dihalogenated aromatic compound to the dihalogenated cinnamic acid is 80-99:1-20; The molar ratio of the dihalogenated aromatic compound and the dihalogenated cinnamic acid to the ionic sulfur is 0.99-1.01:1.

00.

6. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: firstly subjecting a sulfur-containing monomer to a dehydration reaction in an organic polar solvent and optionally a base under the protection of an inert gas or nitrogen; then adding a dihalogenated aromatic compound and a dihalogenated cinnamic acid treated with light or not treated with light to react at 200-250° C. for 2-6 hours; then reacting at 250-300° C. for 2-6 hours; then cooling, collecting the synthesized resin, washing, drying, and optionally subjecting the resin to light treatment, so as to obtain the cinnamic acid-modified polyarylene sulfide.

7. The preparation method according to claim 1, characterized in that: The organic polar solvent is selected from at least one of N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide or sulfolane.

8. The preparation method according to claim 1, characterized in that: The method also includes extruding and granulating the obtained cinnamic acid-modified polyarylene sulfide.

9. A cinnamic acid-modified polyarylene sulfide, characterized in that: Prepared by the method according to any one of claims 1 to 8.

10. A cinnamic acid-modified polyarylene sulfide membrane, characterized in that: The cinnamic acid-modified polyarylene sulfide film is prepared as follows: the cinnamic acid-modified polyarylene sulfide of claim 9 is prepared into a cinnamic acid-modified polyarylene sulfide film by a casting method.